Metallic Materials - Selected Standards: Manual

Download as pdf or txt
Download as pdf or txt
You are on page 1of 102

MANUAL

METALLIC MATERIALS - SELECTED STANDARDS

DEP 30.10.02.11-Gen.

November 1994
(DEP Circular 35/98 has been incorporated)

DESIGN AND ENGINEERING PRACTICE

USED BY
COMPANIES OF THE ROYAL DUTCH/SHELL GROUP

This document is confidential. Neither the whole nor any part of this document may be disclosed to any third party without the prior written consent of Shell Internationale
Petroleum Maatschappij B.V., The Hague, the Netherlands. The copyright of this document is vested in Shell Internationale Petroleum Maatschappij B.V., The Hague,
the Netherlands. All rights reserved. Neither the whole nor any part of this document may be reproduced, stored in any retrieval system or transmitted in any form or by
any means (electronic, mechanical, reprographic, recording or otherwise) without the prior written consent of the copyright owner.
PREFACE
DEPs (Design and Engineering Practice) publications reflect the views, at the time of publication, of:
Shell Global Solutions International B.V. (Shell GSI)
and
Shell International Exploration and Production B.V. (SIEP)
and
Shell International Chemicals B.V. (SIC)
and
other Service Companies.
They are based on the experience acquired during their involvement with the design, construction, operation and
maintenance of processing units and facilities, and they are supplemented with the experience of Group Operating
companies. Where appropriate they are based on, or reference is made to, international, regional, national and industry
standards.
The objective is to set the recommended standard for good design and engineering practice applied by Group
companies operating an oil refinery, gas handling installation, chemical plant, oil and gas production facility, or any other
such facility, and thereby to achieve maximum technical and economic benefit from standardization.
The information set forth in these publications is provided to users for their consideration and decision to implement.
This is of particular importance where DEPs may not cover every requirement or diversity of condition at each locality.
The system of DEPs is expected to be sufficiently flexible to allow individual operating companies to adapt the
information set forth in DEPs to their own environment and requirements.
When Contractors or Manufacturers/Suppliers use DEPs they shall be solely responsible for the quality of work and the
attainment of the required design and engineering standards. In particular, for those requirements not specifically
covered, the Principal will expect them to follow those design and engineering practices which will achieve the same
level of integrity as reflected in the DEPs. If in doubt, the Contractor or Manufacturer/Supplier shall, without detracting
from his own responsibility, consult the Principal or its technical advisor.
The right to use DEPs is granted by Shell GSI, SIEP or SIC, in most cases under Service Agreements prim arily with
companies of the Royal Dutch/Shell Group and other companies receiving technical advice and services from Shell GSI,
SIEP, SIC or another Group Service Company. Consequently, three categories of users of DEPs can be distinguished:
1) Operating companies having a Service Agreement with Shell GSI, SIEP, SIC or other Service Company. The
use of DEPs by these operating companies is subject in all respects to the terms and conditions of the relevant
Service Agreement.
2) Other parties who are authorized to use DEPs subject to appropriate contractual arrangem ents (whether as part
of a Service Agreement or otherwise).
3) Contractors/subcontractors and Manufacturers/Suppliers under a contract with users referred to under 1) or 2)
which requires that tenders for projects, materials supplied or - generally - work performed on behalf of the said
users comply with the relevant standards.
Subject to any particular terms and conditions as may be set forth in specific agreements with users, Shell GSI, SIEP
and SIC disclaim any liability of whatsoever nature for any dam age (including injury or death) suffered by any company
or person whomsoever as a result of or in connection with the use, application or implem entation of any DEP,
combination of DEPs or any part thereof, even if it is wholly or partly caused by negligence on the part of Shell GSI,
SIEP or other Service Company. The benefit of this disclaimer shall inure in all respects to Shell GSI, SIEP, SIC and/or
any company affiliated to these companies that may issue DEPs or require the use of DEPs.
Without prejudice to any specific terms in respect of confidentiality under relevant contractual arrangements, DEPs shall
not, without the prior written consent of Shell GSI and SIEP, be disclosed by users to any company or person
whomsoever and the DEPs shall be used exclusively for the purpose for which they have been provided to the user.
They shall be returned after use, including any copies which shall only be made by users with the express prior written
consent of Shell GSI, SIEP or SIC. The copyright of DEPs vests in Shell GSI and SIEP. Users shall arrange for DEPs to
be held in safe custody and Shell GSI, SIEP or SIC may at any time require information satisfactory to them in order to
ascertain how users implement this requirement.
All administrative queries should be directed to the DEP Administrator in Shell GSI.
TABLE OF CONTENTS
1. INTRODUCTION .................................................................................................... 4
1.1 SCOPE .................................................................................................................. 4
1.2 DISTRIBUTION, INTENDED USE AND REGULATORY CONSIDERATIONS......... 4
1.3 STANDARDS ......................................................................................................... 4
1.4 CATEGORIES OF METALS ................................................................................... 5
1.5 SEQUENCE OF MATERIALS ................................................................................ 5
1.6 SPECIFICATION OF MATERIALS ......................................................................... 5
1.7 METAL TEMPERATURE LIMITS ........................................................................... 5
1.8 CHEMICAL COMPOSITION ................................................................................... 6
1.9 DEFINITIONS ........................................................................................................ 6
2. FERROUS METALS - UNALLOYED ................................................................... 9
2.1 PLATES, SHEETS AND STRIP .............................................................................. 9
2.2 TUBES AND TUBING .......................................................................................... 11
2.3 PIPE .................................................................................................................... 12
2.4 FORGINGS, FLANGES AND FITTINGS............................................................... 14
2.5 CASTINGS........................................................................................................... 15
2.6 BARS, SECTIONS AND WIRE ............................................................................. 16
2.7 BOLTING ............................................................................................................. 17
3. FERROUS METALS - ALLOYED ...................................................................... 18
3.1 PLATES, SHEETS AND STRIP ............................................................................ 18
3.2 TUBES AND TUBING .......................................................................................... 23
3.3 PIPE .................................................................................................................... 28
3.4 FORGINGS, FLANGES AND FITTINGS............................................................... 34
3.5 CASTINGS........................................................................................................... 43
3.6 BARS, SECTIONS AND WIRE ............................................................................. 47
3.7 BOLTING ............................................................................................................. 49
4. NON-FERROUS METALS ................................................................................... 53
4.1 PLATES, SHEETS AND STRIP ............................................................................ 53
4.2 TUBES AND TUBING .......................................................................................... 57
4.3 PIPE .................................................................................................................... 61
4.4 FORGINGS, FLANGES AND FITTINGS............................................................... 65
4.5 CASTINGS........................................................................................................... 68
4.6 BARS, SECTIONS AND WIRE ............................................................................. 70
4.7 BOLTING ............................................................................................................. 73
5. REFERENCES..................................................................................................... 74

APPENDICES
APPENDIX 1 LOW TEMPERATURE (LT) STEELS FOR USE WITH DEP 30.10.02.31-
Gen. ............................................................................................................ 76
1. INTRODUCTION

1.1 SCOPE
This DEP specifies appropriate standards for metallic construction materials. It is a
revision of, and replaces, the DEP of the same number and title dated October 1982.
By identifying alternative materials standards, this DEP has two main functions, as
follows:
 Where a particular materials standard is specified for certain equipment (e.g. in a
DEP), if the Contractor wishes to propose an alternative (equivalent) material he may
use this DEP to select a suitable materials standard which would normally be
acceptable to the Principal. Note, however, that such substitution shall not be made
automatically and still requires the approval of the Principal.
 In situations where required materials are not explicitly specified, this DEP may be
invoked to act as a basis for the Contractor's materials selection.
It should be realized that materials may fail owing to undesirable properties being induced
during fabrication and/or service, such as metallurgical changes or corrosion of various
types. Such factors shall be taken into account when selecting a material for a given
service. Measures which may be required to prevent or limit such risks (e.g. special heat
treatment) are outside the scope of this DEP and are not indicated. The materials
engineer should therefore be consulted regarding selection of materials.

1.2 DISTRIBUTION, INTENDED USE AND REGULATORY CONSIDERATIONS


Unless otherwise authorised by SIPM, the distribution of this DEP is confined to
companies forming part of the Royal Dutch/Shell Group or managed by a Group
company, and to Contractors nominated by them (i.e. the distribution code is "C", as
described in DEP 00.00.05.05-Gen.).
This DEP is intended for use in oil refineries, chemical plants, gas plants, exploration and
production facilities and supply/marketing installations.
If national and/or local regulations exist in which some of the requirements may be more
stringent than in this DEP, the Contractor shall determine by careful scrutiny which of the
requirements are the more stringent and which combination of requirements will be
acceptable as regards safety, environmental, economic and legal aspects. In all cases the
Contractor shall inform the Principal of any deviation from the requirements of this DEP
which is considered to be necessary in order to comply with national and/or local
regulations. The Principal may then negotiate with the Authorities concerned with the
object of obtaining agreement to follow this DEP as closely as possible.

1.3 STANDARDS
This DEP identifies materials to ASTM standards with reference to various other
standards. All series of standards rank equally, although individual specifications may not
be identical.
The choice of standard, therefore, is optional and depends on practical circumstances,
such as the location where the plant is to be erected, the acceptability of the standard
under the applicable design/construction code and the availability and economy of the
material.
In order to avoid confusion and to provide a consistent basis for the basic specification of
the materials, only one series of standards should be used for any particular piece of
equipment (i.e. avoid mixing ASTM standards with JIS standards, etc.).
Where a deviation from this rule is required, agreement shall be obtained from the
Principal.
The use of trade names for materials shall be avoided whenever an authoritative
specification reference is available.
NOTES: 1. Where metric versions of ASTM standards are available (e.g. ASTM A278M) they should be
selected. In most cases, ASTM standards and their metric version are issued as a single standard
(e.g. ASTM A182/A182M).
2. When BS, DIN or AFNOR standards are replaced by EN standards, the EN standard shall be
considered equivalent.

1.4 CATEGORIES OF METALS


The following categories of metals are covered by this DEP:
 Ferrous metals - unalloyed
 Ferrous metals - alloyed
 Non-ferrous metals
In each category the following products are dealt with:
 Plates, sheets and strip;
 Tubes and tubing;
 Pipe;
 Forgings, flanges and fittings;
 Castings;
 Bars, sections and wire;
 Bolting.

1.5 SEQUENCE OF MATERIALS


The sequence of materials in the column "Designation and Application" in Sections 2, 3
and 4 is generally such that the subsequent number indicates a material with an increase
in the concentration and/or number of the alloying elements.

1.6 SPECIFICATION OF MATERIALS


Materials standards identified on drawings, requisition sheets or other documents shall be
specified fully in accordance with the information given in Sections 2, 3 and 4, including all
additional requirements applicable to the standard. For materials covered by the MESC
system, the additional requirements stated therein shall also be met.
The latest issue of the selected materials standard shall be used. As this latest issue
(including amendments) always prevails, the year of issue of the standard need not be
shown.

1.7 METAL TEMPERATURE LIMITS


The temperature limits shown in Sections 2, 3 and 4 are approximate limits allowed for
the average temperature through the cross-section of the construction material during
normal operation.
The values mentioned should be regarded as an indication only and do not
necessarily apply to cases where corrosion and/or conditions which may affect the
structure of the material occur.
It should be noted that the indicated temperature limits do not necessarily exclude the
application of the materials beyond these limits, especially for non-pressure-retaining
parts such as internal parts of columns, baffles of heat exchangers, supporting structures,
etc.
Temperatures shown in brackets, e.g. (+400), are unusual for the indicated application
but are allowable from a materials point of view, if so required.
Special attention should be given to the specification and application of metals for service
at low temperatures (metal temperature -20 °C or lower), for which reference shall be
made to Appendix 1 of this specification and to DEP 30.10.02.31-Gen. The materials
engineer should be consulted if there is any doubt on the choice of material for
extreme service temperatures.

1.8 CHEMICAL COMPOSITION


Chemical composition requirements relate to product analyses.
Percentage compositions are by mass.

1.9 DEFINITIONS

1.9.1 General definitions


The Contractor is the party which carries out all or part of the design, engineering,
procurement, construction, commissioning or management of a project or operation of a
facility. The Principal may undertake all or part of the duties of the Contractor.
The Manufacturer/Supplier is the party which manufactures or supplies equipment and
services to perform the duties specified by the Contractor.
The Principal is the party which initiates the project and ultimately pays for its design and
construction. The Principal will generally specify the technical requirements. The Principal
may also include an agent or consultant authorised to act for, and on behalf of, the
Principal.
The word shall indicates a requirement.
The word should indicates a recommendation.
1.9.2 Specific definitions
bar Round, square, rectangular, oval, half-round and half-oval products,
usually ordered in random lengths.

bolting Fastening element provided with thread.

(headed) bolt:
Fastening element with a head (usually hexagonal) at one end, the
other end being threaded to take a nut.

stud bolt:
Fastening element, generally with continuous thread, to be used with
nuts at both ends.

stud:
Fastening element with discontinuous thread, one end threaded to be
screwed into a body, the other end threaded to take a nut.

nut:
Fastening element provided with female thread.

casting Product obtained by pouring molten metal into a mould.

flanges and Standard piping components other than tube/pipe, valves, bolting and
fittings gaskets.

forging Metal product, hot worked or hot stamped into a desired shape.

pipe Tubular product; sizes up to and including DN 300 indicated by a


nominal size roughly corresponding to the inside diameter; sizes larger
than DN 300 indicated by the outside diameter. Pipe is usually ordered
in random lengths.

plate Flat product, minimum thickness approximately 6 mm and minimum


width approximately 300 mm.

section A shape that is long in relation to its cross-sectional dimensions,


having a cross section other than those of wire, rod, bar, tube, tubing
and pipe, such as L, U, I, T, etc.

sheet Flat product, thickness less than 6 mm and minimum width


approximately 300 mm.

strip Flat product, maximum width approximately 300 mm and maximum


thickness approximately 1/6 of the width.

tube Tubular product, indicated by the outside diameter and usually ordered
cut to a specific length.

tubing Tubular product of small diameter, indicated by the outside diameter


and usually ordered in long lengths.

wire Round product, usually ordered in long lengths.


1.9.3 Abbreviations
AFNOR Association Française de Normalisation

ASTM American Society for Testing and Materials


BS British Standard

DIN Deutsches Institut für Normung

ISO International Organization for Standardization

JIS Japanese Industrial Standard


2. FERROUS METALS - UNALLOYED

2.1 PLATES, SHEETS AND STRIP


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
2.1.1 Carbon steel sheets +100 A 446 - A/ 2989-Z22/ 17162-2: - - 4998:
of structural quality, G165 G600 St E250-2Z Z600-220
galvanized Gruppe
For general use 600
2.1.2 Carbon steel plates (+350) A 283 - C EN10025: EN 10025: EN10025: G 3106 630 - 1) To be killed or
of structural quality 1) Fe 430B Fe 430B Fe 430B SM 400 Fe 430B semi-killed.
up to 50 mm C content B or C
thickness 0.23% max. 1)
For non-pressure-
retaining parts
2.1.3 Carbon steel plates of (+350) A 283 - C EN10025: EN 10025: EN10025: G 3106 630 - 1) For further
structural quality 2) Fe 430B Fe 430B Fe 430B SM 400 Fe 430B reference
For standard C content B or C see DEP
vertical storage 0.23% max. 2) 34.51.01.31-
tanks with Gen.
internal pressure 2) To be killed or
up to 54 mbar semi-killed.
(546 mm water
column) and
vacuum up to
6.2 mbar (64 mm
water column)
1)
2.1.4 Carbon steel plates +400 A 285 - C 1501: 151 - 17155: H II A 36-205 G 3103 2604-4 1) Replace suffix
(killed or semi-killed) 2) 400B/430B 2) A 42 CP SB 410 P7/P9 B with A if
up to 50 mm C content 1) 2) C content guaranteed
thickness - low 0.23% max. 0.23% elevated
strength max. temper-ature
For pressure- Mn may properties are
retaining parts be not required.
increased 2) To be killed or
to 1.30% semi-killed.
max.
or
G 3115
SPV 235
2.1.5 Carbon steel plates +400 A 515 - 1501: 161 - 17155: H II A 36-205 G 3103 2604-4 1) Replace suffix
(Si-killed) - 60/65 400B/430B 2) A 42 CP SB 410 P7/P9 B with A if
low/medium strength C content 1) 2) C content guaranteed
For pressure- 0.23% 0.23% elevated
retaining parts max. max. temper-ature
Mn may properties are
be not required.
increased 2) To be Si-killed.
to 1.30%
max.
or
G 3115
SPV 235
2.1.6 C-Mn steel plates +400 A 515 -70 1501: 17155: A 36-205 G 3103 2604-4 1) For tube sheets
(Si-killed) - 1) 223-490B 19 Mn 6 A 52 CP SB 480 P16/P18 to be welded to
medium/high strength or 3) or tubes, see
For tube sheets 1501: G 3115 2.1.7.
not welded to 224-490B SPV 315 For tube sheets
shell and/or tubes 1) 2) to be welded to
shell, see 2.4.3.
2) Replace suffix
B with A if
guaranteed
elevated
temper-ature
properties are
not required.
3) To be Si-killed.
2. FERROUS METALS - UNALLOYED (Cont'd)

2.1 PLATES, SHEETS AND STRIP (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
2.1.7 C-Mn steel plates +400 A 299 1501: 17155: A 36-205 G 3115 2604-4 1) For tube sheets
(killed or semi-killed) - 1) 223-490B or 19 Mn 6 A 52 CP SPV 355 P18 to be welded to
high strength C content 1501: 3) shell, see 2.4.3.
For pressure- 0.23% max. 224-490B 2) Replace suffix
retaining parts Mn content 1) 2) B with A if
and for tube 1.30% max. guaranteed
sheets to be elevated
welded to tubes temperature
properties are
not required.
3) To be killed or
semi-killed.
2.1.8 Fine-grained C-Mn +400 A 516 - 1501: 224- 17102: A 36-205 G 3126- 2604-4 1) For low-
steels - low strength 1) 6) 55/60 400 A/B or T St E 285/ A 37/A 42 SLA P9 temperature
For pressure- C content 430 A/B T St E 315 FP 235B/ applications,
retaining parts 0.23% max. 2) 3) 4) 4) 5) 4) 5) SLA-325A see Appendix 1
also at low 4) and DEP
temperatures A 662 - A 30.10.02.31-
4) Gen.
2) Use suffix A if
guaranteed
elevated
temperature
properties are
not required.
Use suffix B if
guaranteed
elevated
temperature
properties are
required.
2.1.9 Fine-grained C-Mn +400 A 516 - 65 1501: 17102: A 36-205 - 2604-4
steels - medium 1) 6) C content 224-460 A/B T St E 355 A 48 FP P15
strength 0.23% max. 2) 3) 4) 4) 4) 5)
For pressure-
retaining parts
also at low
temperatures A 662 - B
4)
2.1.10 Fine-grained C-Mn +400 A 537 - 1501: 17102: A 36-205 - - 3) The suffix LT
steels - high strength 1) 6) Class 1 224-490 A/B T St E 380 A 52 FP followed by a
For pressure- (Normalized 2) 3) 4) 4) 4) 5) number shall be
retaining parts ) added if impact
also at low 4) tests at or
temperatures below 0 °C are
(Use subject to required.
specific (The number
approval) indicates the
impact test
temperature -
see BS 1501)
4) For tube sheets
to be welded
to shell, see
2.4.3.
2.1.11 Fine-grained C-Mn +400 A 537 - - 17102: - - - 5) To be killed or
steels - very high 6) Class 2 E St E 460 semi-killed.
strength (Q/T) 6) Specify
For pressure- V+Ti+Nb <
retaining parts 0.15%
(Use subject to
specific
approval.)
2. FERROUS METALS - UNALLOYED (Cont'd)

2.2 TUBES AND TUBING


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
2.2.1 Electric-resistance- +400 A 214 3606: 17177: A 49-142 G 3461 2604-3 1) A non-
welded carbon steel 1) 4) ERW 320 St 37.8 TS E185A STB 340 TW5 destructive
tubes 1) 4) 1) 1) ERW 1) 4) electric test in
For unfired heat 1) accordance
transfer with the
equipment requirem ents of
ASTM A450 or
equivalent shall
be
2.2.2 Seamless cold-drawn +400 A 179 3606: 17175: A 49-215 G 3461 2604-2 carried out in
carbon steel tubes 2) 1) 4) CFS 320 St 35.8 III TU 37-C STB 340 TS5 addition to the
For unfired heat 1) 1) 1) Seamless 1) hydrostatic
transfer 1) test.
equipment 2) For low-
temperature
2.2.3 Electric-resistance- +400 A 178 - A 3059: Part 1 17177: A 49-243 G 3461 2604-3 applications,
welded carbon steel 1) 3) 4) 5) - St 37.8 TS 37-C STB 340 TW5 see Appendix 1
tubes ERW 320 1) 3) 5) 1) 3) 5) ERW 1) 3) 4) 5) and DEP
For boilers and 1) 3) 4) 5) 1) 3) 5) 30.10.02.31-
superheaters Gen.
3) Electric-
resistance-
welded tube
may be used
up to and
including
102 mm
external
diameter.
2.2.4 Electric-resistance- +400 A 226 3059: Part 2 17177: A 49-243 G 3461 2604-3 4) To be killed or
welded carbon steel 1) 3) 5) - St 37.8 TS 37-C STB 340 TW5 semi-killed.
tubes (Si-killed) ERW-2 360 1) 3) 5) 1) 3) 5) ERW 1) 3) 4) 5) 5) Specify
For boilers and Cat. 2 1) 3) 5) elevated
superheaters at 1) 3) 5) temperature
high working properties.
pressures
2.2.5 Seamless carbon +400 A 192 3059: Part 2 17175: A 49-213 G 3461 2604-2
steel tubes (Si-killed) 1) 5) - St 35.8 III TU 37-C STB 340 TS5
For boilers and S2 360 1) 5) 1) 5) Seamless 1) 5)
superheaters at Cat. 2 1) 5)
high working 1) 5)
pressures
2.2.6 Seamless carbon +400 A 334-6 3603: 17173: A 49-215 G 3464 2604-2
steel tubes (Si-killed) 2) C content CFS 430 LT TT St 35 N TU 42BT STBL 380 TS10
For unfired heat 0.23% 1) 1) 1) C content 1)
transfer max. 0.23%
equipment 1) max.
operating at low 1)
service
temperatures
2. FERROUS METALS - UNALLOYED (Cont'd)

2.3 PIPE
DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
2.3.1 Galvanized seamless +50 - - 2440 - - 65 1) Galvanized pipe
carbon steel pipe 1) 2) 1) 1) with screwed
For air and water connections
lines only only.
2) Specify
seamless API
5L-B pipe with
NPT threaded
couplings,
galvanized to
ASTM A53,
para 19.
2.3.2 Electric-resistance- +350 - 3601: 1626 A 49-242 G 3454 2604-3 1) Specify API 5L-
welded carbon steel 1) 2) ERW 430 St 44.0 TS E290 STPG TW9 B electric-
pipe 2) 2) 410 2) resistance
For outside plot 2) welded pipe.
product lines, C content
except lines 0.23% max.
carrying Mn may be
hazardous increased to
products, 1.30% max.
including 2) To be killed or
hydrocarbons semi-killed.
lighter than
gasoline
2.3.3 Electric-fusion- +400 A 672 - - - - - -
welded carbon steel C 65
pipe, sizes larger than Class 32
DN 400 C content
For inside plot 0.23%
product lines max.
2.3.4 Seamless carbon +400 - 3601: S430 - A 49-211 - 2604-2 1) Specify API
steel pipe 1) 2) 2) TU E250 TS 9 5L-B seamless
For most inside B 2) pipe with C
plot product and 2) content
utility lines. 0.23% max.
(For certain Mn may be
specific services, increased to
ASTM A106-B 1.30% max.
pipe to be used - Pipe shall be
see 2.3.6.) furnished in the
normalized
condition.
2) To be killed or
semi-killed.
Seamless usually
not obtainable in
sizes larger than
DN 400. For larger
sizes see 2.3.5.
2. FERROUS METALS - UNALLOYED (Cont'd)

2.3 PIPE (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., ASTM BS DIN AFNOR JIS ISO REMARKS
°C (See
1.7)
2.3.5 Submerged arc welded +400 - - - - - - 1) Specify API 5L
carbon steel pipe, sizes 1) 2) -B subm erged-
larger than DN 400 arc welded pipe
For inside plot with
product and utility C content
lines 0.23% max.
Mn may be
increased to
1.30% max.
Pipe shall be
furnished in the
normalized
condition.
2) To be killed or
semi-killed.

2.3.6 Seamless C-Mn steel +400 A 106 -B 3602: 17175: A 49-211 G 3455 2604-2 1) To be killed or
pipe (Si-killed) C content HFS 430 St 45.8 I TU E250 STS 410 TS 5 or semi-killed.
For inside plot 0.23% max., Cat. 2 III Normalized (350 C max.)
TS 9H
piping, for special Mn may be Normalized Normalized 1) C content Normalized Seamless usually
services (such as increased to 0.23% max. not obtainable in
hydrocarbon + 1.30% max. Normalized sizes larger than
hydrogen, Normalized DN 600. For larger
hydrocarbon + A 49-213 G 3456 sizes use ASTM
sulphur compounds, TU 42C STPT 410 A672 C65
fuel gas). Normalized C content Class 32
For seamless shells 0.23% max. (see 2.3.3)
of vessels, for Normalized
welded-on nozzles,
for welded furnace
coils and for certain
special applications

2.3.7 Seamless fine-grained (+400) A 333 - 3603: - A 49-230 G 3460 2604-2 1) For low-
C-Mn steel pipe 1) 2) Grade 6 HFS 430LT TU 42 BT STPL 380 TS 10 temperature
(Si-killed) C content C content applications,
For process lines at 0.23% max., 0.23% max. see Appendix 1
low service Mn may be and DEP
temperatures increased to 30.10.02.31
1.30% max. -Gen.
2) Specify
V+Ti+Nb <
0.15%
Seamless usually
not obtainable in
sizes larger than
DN 400. For larger
sizes use ASTM
A671, CC65,
Class 32
(see 2.3.8)

2.3.8 Electric-fusion-welded (+400) A 671 - - - - - - 1) For low-


fine-grained C-Mn steel 1) 2) CC65 temperature
pipe (Si-killed), sizes Class 32 applications,
larger than DN 400 C content see Appendix 1
For process lines at 0.23% max., and DEP
moderate or low Mn may be 30.10.02.31-
service increased to Gen.
temperatures 1.30% max. 2) Specify
V+Ti+Nb <
0.15%
2. FERROUS METALS - UNALLOYED (Cont'd)

2.4 FORGINGS, FLANGES AND FITTINGS


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
2.4.1 Carbon steel butt- +400 A 234 - 1640: WPB - - - - Sizes up to DN 400
welding pipe fittings WPB or C content incl. shall be
For general use WPBW 0.23% max. seamless.
C content Mn may be Larger sizes may
0.23% increased to be either seamless
max. 1.30% max. or welded.
Mn may be Normalized
increased
to 1.30%
max.
Normalized
2.4.2 Carbon steel butt- (+400) A 420 - 1640: WPLO - - - - Sizes up to DN 400
welding pipe fittings 1) WPL6 or C content incl. shall be
For low service WPL6W 0.23% max. seamless.
temperature C content Mn may be Larger sizes may
0.23% increased to be either seamless
max. 1.30% max. or welded.
Mn may be Normalized
increased 1) For low-
to 1.30% temperature
max. applications,
Normalized see Appendix 1
and DEP
30.10.02.31-
Gen.
2.4.3 Carbon steel forgings +400 A 105 1503: 17243: E 29- G 3202 2604-1
For piping C content 221-460 17Mn4 204 SFVC 2A. F 12 N
components, 0.25% Normalized Normalized BF48N C content
including flanges, max., 0.25% max.
fittings, valves and Mn may be Mn may be
other pressure- increased increased
retaining parts and to 1.20% to
also for tube sheets max. 1.20% max.
to be welded to Normalized Normalized
shell
2.4.4 Carbon steel forgings +400 A 266 - - - - - - -
For pressure vessel Class 2
components and C content
associated pressure- 0.25%
retaining equipment, max.
including tube Normalized
sheets
2.4.5 Carbon-manganese (+400) A 350 - 1503: - - G 3205 - 1) For low-
steel forgings 1) LF2 224-430LT40 SFL 2 temperature
For piping C content Normalized C content applications,
components, 0.23% 0.23% max. see Appendix 1
including flanges, max. Normalized and DEP
fittings, valves and Normalized 30.10.02.31-
other pressure- Gen.
retaining parts at
low service
temperatures
2.4.6 Carbon-manganese +350 A765 - - - - - - 1) For low-
steel forgings 1) Grade II temperature
For pressure vessel C content applications,
components and 0.23% see Appendix 1
associated presure- max. and DEP
retaining equipment, 30.10.02.31-
including tube Gen.
sheets, at low
service temperatures
2. FERROUS METALS - UNALLOYED (Cont'd)

2.5 CASTINGS
DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
2.5.1 Grey iron castings +350 A 48 1452: 220 1691: GG A 32-101 G 5501 185: 1) Cast iron not to
For non-pressure- Class 30 25 FGL 250 FC 250 250 be used in
retaining (internal) hazardous
parts A 48 1452: 300 F 32-101 G 5501 185: service or
Class 40 1691: GG FGL 300 FC 300 300 above 10 bar.
30 2) Mechanical
2.5.2 Grey iron castings +650 A 319 - - - - - - properties may
For non-pressure- Class II be improved by
retaining (internal) the addition of
parts at elevated certain
temperatures elem ents, such
as Cr and Ni
(i.e. "pearlitic
cast iron").
2.5.3 Grey iron castings +350 A 278 1452: 300 1691: GG A 32-101 G 5501 185:
For pressure- Class 40 1) 2) 30 FGL 300 FC 300 300
retaining parts and 1) 2) 1) 2) 1) 2) 1) 2)
cooler channels
2.5.4 Ductile iron castings +400 A 395 2789: 400/18 1693: A 32-201 G 5502 1083: 1) Metallographic
For pressure- 1) 2) GGG 40 FGS FCD 400 400/18 examination in
retaining parts 400/18 2) accordance
including fittings and 2) with ASTM
valves A395 shall be
made
additionally to
the tensile test.
2) Hardness test
and 0.2% proof
test to be
included in test-
ing programme.
2.5.5 Steel castings (+400) A 216 - 1504: 17245: A 32-055 G 5151 - 1) For low-
For pressure- WCA 161-430A GS-C25 A 420 SCPH1 temperature
retaining parts WCB* 161-480A* CP-M SCPH2* applications,
WCC 161-480A* A 480 see Appendix 1
* C content * C content CP-M *C and DEP
0.25% max. 0.25% max. content 30.10.02.31-
0.25% Gen.
max.
Mn may
be
increased
to 1.20%
max.

2.5.6 Steel castings (+400) A 352 - 1504: SEW 685 A 32-055 G 5152 -
For pressure- 1) LCB* 161- GS-21Mn5 A 420 SCPL1*
retaining parts at 430ALT40 FP-M
low service A 480 *C
temperatures LCC FP-M content
0.25%
* C content max.
0.25% max. Mn may
be
increased
to 1.20%
max.
2. FERROUS METALS - UNALLOYED (Cont'd)

2.6 BARS, SECTIONS AND WIRE


DESIGNATION AND Metal
APPLICATION Temp., ASTM BS DIN AFNOR JIS ISO REMARKS
°C (See
1.7)
2.6.1 Carbon steel bars, +350 A 36 EN 10 025: EN 10 025: EN 10 G 3106 630 1) For non-welded
sections and raised- C content Fe 430B Fe 430B 025: SM 400B Fe 430B items, and for
tread plates of 0.23% max. Fe 430B or C items that will
structural quality 1) 2) 2) not be welded,
For general restriction on C
structural content may be
purpose disregarded.
2) To be killed or
semi-killed.
2.6.2 Low-carbon steel +400 A 576 - 970: 080 A20 17200: A 35-552 G 4051 - 1) To be killed or
bars 1022 1) Ck 22 XC 18 S22C semi-killed.
For machined 1) 2) 2) Where free-
parts machining
quality is
required
specify Grade
1117.
2.6.3 Medium-carbon steel +400 A 576 - 970: 17200: A 35-552 G 4051 683-1 1) To be killed or
bars 1035 080 A35 Ck 35 XC 38 S35C C35 semi-killed.
For machined 1045 080 A47 Ck 45 H1 S45C C45 2) Where free-
parts 1055 080 A57 Ck 55 XC 48 S55C C55 machining
1) 2) 1) H1 quality is
XC 55 required
H1 specify Grade
1137.
2.6.4 High-carbon steel +230 A 689/A 970: 060 A96 - - - - 1) To be killed or
bars 576 1) semi-killed.
For springs 1095
1)
2.6.5 Music spring quality +230 A 228 5216 - - - -
steel wire
For springs
2.6.6 Carbon steel bars and (+230) A 36 EN 10 025: EN 10 025: A 35-501 G 3106 630 1) For non-welded
sections C content Fe 430B Fe 430B E 28-2 SM 400B Fe 430B items, and for
For lifting lugs, 0.23% 2) or C items that will
sliding bars etc. max. 2) not be welded,
1) 2) restriction on C
content may be
disregarded.
2) To be killed or
semi-killed.
2. FERROUS METALS - UNALLOYED (Cont'd)

2.7 BOLTING
DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
2.7.1 Carbon steel bolts +230 A 307 - B 1769 - - - - Approved free
For structural machining quality
purposes acceptable.
For bolting to be
used beyond
limits indicated
see 3.7.1.
For nuts
see 2.7.2.
2.7.2 Carbon steel nuts +230 A 563 - A 1769 - - G 4051 -
For bolts S 43C
specified under
2.7.1
2.7.3 Medium-carbon steel +450 A 194 - 2H 4882: 2H 17200: A 35-557 - -
nuts C45 XC 38
For bolting
specified under
3.7.1
3. FERROUS METALS - ALLOYED

3.1 PLATES, SHEETS AND STRIP


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.1.1 0.3 Mo steel plates +500 - 1501: 243 17155: A 36-206 - 2604-4 NOT for hydrogen
For pressure- 1) 15 Mo 3 15 D 3 P26 service.
retaining parts at 1) 1)
high service
temperatures
3.1.2 0.5 Mo steel plates +500 A 204 - - - - G 3103 2604-4 1) Specify total
For pressure-retaining A or B SB 450M P28 Al content
parts at high service or 0.012% max.
temperatures SB 480M
C content
0.20%
max.
1)
3.1.3 Low-alloy nickel- +500 - - - - - - Ordered against
copper- proprietary
molybdenum- specifications
niobium steel subject
plates to agreement.
For boiler drums
3.1.4 Low-alloy (+500) - 1501: 271 - - - -
manganese-
chromium-
molybdenum-
vanadium steel
plates
For boiler drums
3.1.5 1 Cr - 0.5 Mo steel +600 A 387 - 12 1501: 620 17155: A 36-206 G 4109 2604-4 1) For resistance
plates Class 2 2) 3) 13CrMo4 4 15 CD 4- SCMV2 P32 to hydrogen
For high service 2) 3) 2) 3) 4) 05 2) 3) 2) 3) 5) attack, see API
temperatures 2) 3) 5) 941.
and/or resistance 2) To be
to hydrogen normalized and
attack tempered or
1) quenched and
tempered.
3) See below.
4) When
resistance to
hydrogen
attack is
required,
specify
Cr 0.8% min.
5) Specify Mo
0.45% min. for
hydrogen
service.
3) Specify:
Cu 0.20% max.
Ni 0.30% max.
(%Si+%Mn)  1.10
(%Si+%Mn) x (%P+%Sn) x 104  150.
3. FERROUS METALS - ALLOYED (Cont'd)

3.1 PLATES, SHEETS AND STRIP (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.1.6 1.25 Cr - 0.5 Mo steel +600 A 387 - 11 1501: 621 - - G 4109 - 1) For resistance
plates Class 2 2) 3) 4) SCMV3 to hydrogen
For high service 2) 3) 4) 2) 3) 4) attack, see API
temperatures 941.
and/or resistance
to hydrogen 2) Specify to be
attack normalized and
1) tempered or
quenched and
tempered.
3.1.7 2.25 Cr - 1 Mo steel +625 A 387 - 22 1501: 17155: A 36-206 G 4109 2604-4 3) See below
plates Class 2 622-515 10CrMo9 10 CD 9- SCMV4 P34
For high service 2) 3) 2) 3) 10 10 2) 3) 2) 3) 4) Specify
temperatures 2) 3) 2) 3) P 0.005% max.
and/or resistance
to hydrogen
attack
1)
3.1.8 3 Cr - 1 Mo steel +625 A 387 - 21 - - A 36-206 G 4109 -
plates Class 2 10 CD SCMV5
For high service 2) 3) 12-10 2) 3)
temperatures 2) 3)
requiring
optimum creep
resistance and/or
resistance to
hydrogen attack
1)
3.1.9 5 Cr - 0.5 Mo steel +650 A 387 - 5 - - A 36-206 G 4109 - 1) Specify to be
plates Class 2 Z 10 SCMV6 normalized and
For high service 1) CD 5-05 1) tempered or
temperatures 1) quenched and
and/or resistance tempered.
to sulphur
corrosion
3.1.10 0.5 Ni steel plates (+400) - - 17280: A 36-208 - - 1) For low-
For pressure- 1) 13 Mn Ni 6 0.5 Ni 355 temperature
retaining parts at 3 applications,
low service see Appendix 1
temperatures and DEP
30.10.02.31-
Gen.
3.1.11 1.5 Ni steel plates (+400) - - 17280: A 36-208 - 2604-4
For pressure- 1) 14 Ni Mn 6 1.5 Ni 355 P42
retaining parts at
low service
temperatures
3.1.12 3.5 Ni steel plates (+400) A 203 - D 1501: 503 17280: A 36-208 G 3127 2604-4
For pressure- 1) 10 Ni 14 3.5 Ni 285 SL3N255 P43
retaining parts at
low service
temperatures
3.1.13 5 Ni steel plates (+400) - - 17280: A 36-208 G 3127 -
For pressure- 1) 12 Ni 19 5 Ni 390 SL5N590
retaining parts at
low service
temperatures
3) Specify:
Cu 0.20% max.
Ni 0.30% max.
(%Si+%Mn)  1.10
(%Si+%Mn) x (%P+%Sn) x 104  150.
3. FERROUS METALS - ALLOYED (Cont'd)

3.1 PLATES, SHEETS AND STRIP (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.1.14 9 Ni steel plates -200 A 353 1501: 510N 17280: A 36-208 G 3127 2604-4 1) For low
For pressure-retaining 1) 2) 2) X 8 Ni 9 9 Ni 490 SL9N520 P45 temperature
parts at low service NNA 2) 2) (N+N+T) applications,
temperatures 2) 2) see Appendix 1
and
A 553 - 1501: 510 17280: A 36-208 G 3127 2604-4 DEP
Type I 2) X 8 Ni 9 H 9 Ni 585 SL9N590 P45 30.10.02.31-
2) A 2) 2) (Q+T) Gen.
2) 2) 2) Specify
C 0.10% max.
Si 0.30% max.
P 0.002% max.
S 0.005% max.
3.1.15 13 Cr steel plates, sheets +540 A 240 - - 17440: - - - 1) For cladding
and strip Type X 6 Cr 13 purposes only.
For pressure-retaining 410S 1)
parts under certain 1)
corrosive conditions - 17440: - G 4304 - 2) Type 405 shall
A 240 - X 6 CrAl SUS 405 not be used
Type 405 13 1) 2) above 400 °C.
1) 2) 1) 2)
3.1.16 18 Cr-8 Ni steel plates, -200 A 240 - 1501 17440: A 36-209 G 4304 2604-4 1) For low-
sheets and strip (+400) Type 304 304S31 X 5 CrNi Z 7 CN SUS 304 P47 temperature
For pressure-retaining 1) 2) 2) 18 10 18-09 2) 2) applications,
parts at low service 2) 2) see Appendix 1
temperatures or to and DEP
prevent product A 240 - - - A 36-209 G 4304 - 30.10.02.31-
contamination Type Z 6 CN SUS Gen.
304N 18-09 Az 304N1
2) 2) 2)
3.1.17 18 Cr-8 Ni steel plates, -200 A 240 - 1501: 17440: A 36-209 G 4304 2604-4 2) The material
sheets and strip +500 Type 304L 304S11 X 2 CrNi Z 3 CN SUS 304L P46 shall be
For pressure-retaining 1) 2) 2) 19 11 18-10 2) 2) capable of
parts under certain 2) 2) passing the
corrosive conditions Practice E
and/or low and intergranular
moderate service corrosion test
temperatures as specified in
ASTM A262.
3.1.18 18 Cr-8 Ni stabilized steel (-100) A 240 - 1501: 17440: A 36-209 G 4304 2604-4 3) For optimum
plates, sheets and strip +600 Type 321 321S31 X 6 CrNiTi Z 6 CNT SUS 321 P53 resistance to
For pressure-retaining 2) 3) 2) 3) 18 10 18-10 2) 3) 2) 3) intergranular
parts under certain 2) 3) 2) 3) corrosion,
corrosive conditions specify a
and/or high service A 240 - 1501: 17440: A 36-209 G 4304 2604-4 stabilization
temperatures Type 347 347S31 X 6 CrNiNb Z 6 CNNb SUS 347 P50 heat treatment
2) 3) 2) 3) 18 10 18-10 2) 3) 2) 3) at
2) 3) 2) 3) 950 °C, subse-
quent to
solution heat
treatment.
3.1.19 18 Cr-10 Ni-2 Mo steel -200 A 240 - 1501: 17440: A 36-209 G 4304 2604-4
plates, sheets and strip +500 Type 316 316S31 X5 Z 7 CND SUS 316 P60
For pressure-retaining 1) 2) 2) CrNiMo 17 17-11-02 2) 2)
parts under certain 12 2 2)
corrosive conditions 2)
and/or high service A 240 - 1501: A 36-209 G 4304 2604-4
temperatures Type 316L 316S11 17440: Z 3 CND SUS 316L P57
2) 2) X2 17-11-02 2) 2)
CrNiMo 17 2)
13 2
2)
3. FERROUS METALS - ALLOYED (Cont'd)

3.1 PLATES, SHEETS AND STRIP (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.1.20 18 Cr-10 Ni-2 Mo (-200) A 240 - 1501: 17440: A 36-209 - - 1) The material
stabilized steel plates, +500 Type 316Ti 320S31 X6 Z 6 CNDT shall be
sheets and strip 1) 2) 1) 2) CrNiMoTi 17-12 capable of
For pressure-retaining 17 12 2 1) 2) passing the
parts under certain 1) 2) Practice E
corrosive conditions A 240 - - A 36-209 - - intergranular
and/or high service Type 17440: Z6 corrosion test
temperatures 316Cb X6 CNDNb as specified in
1) 2) CrNiMoNb 18-12 ASTM A262.
17 12 2 1) 2)
1) 2)
3.1.21 18 Cr-10 Ni-3 Mo steel (-200) A 240 - - - - G 4304 - 2) For optimum
plates, sheets and strip +500 Type 317 SUS 317 resistance to
For pressure-retaining 1) 1) intergranular
parts under certain corrosion,
corrosive conditions specify a
and/or high service G 4304 stabilization
temperatures A 240 - - 17440: A 36-209 SUS 317L - heat treatment
Type 317L X2 Z 3 CND 1) at 950 °C,
1) CrNiMo 18 19-15-04 subsequent to
16 4 1) solution heat
1) treatment.
3.1.22 25 Cr-20 Ni steel plates, +1000 A 240 - 1501: - - G 4304 -
sheets and strip Type 310S 310S16 SUS
For pressure-retaining 310S
parts under certain
corrosive conditions
and/or extreme service
temperatures
3.1.23 18 Cr-8 Ni steel plates, +700 A 240 - 1501: - A 36-209 - 2604-4 1) Specify
sheets and strip Type 304H 304S51 Z 6 CN P48 C 0.06% max.
For pressure-retaining 1) 1) 18-09 1) and Mo+Ti+Nb
parts at extreme 1) 0.4% max.
service temperatures
under certain
corrosive conditions
3.1.24 22 Cr-5 Ni-Mo-N steel (-30) A 240 - 1501: SEW 400: A 36-209 G 4304 - 1) For low
plates, sheets and strip +300 S31803 318S13 X2 Z 3 CND SUS 329J temperature
For pressure-retaining 1) 2) 2) CrNiMo N 22-05 Az 2L applications,
parts under certain 22 5 3 2) 2) etc.
corrosive conditions 2) 2) N 0.15% min.
3.1.25 25 Cr-7 Ni-Mo-N steel (-30) A 240 - - - A 36-209 - -
plates, sheets and strip +300 S32750 Z 3 CND
For pressure-retaining 1) 25-07 Az
parts under certain
corrosive conditions
3.1.26 20 Cr-18 Ni-6 Mo-Cu-N (-200) A 240 - - - - - -
steel plates, sheets and (+400) S31254
strip 1)
For pressure-retaining
parts under certain
corrosive conditions
3. FERROUS METALS - ALLOYED (Cont'd)

3.1 PLATES, SHEETS AND STRIP (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.1.27 Carbon steel or low- A 263 `- - A 36-250 - - 1) Specify base
alloy steel plates with 1) 1) metal and
ferritic stainless steel cladding.
cladding
For high service
temperatures
and/or certain
corrosive
conditions

3.1.28 Carbon steel or low- A 264 - - A 36-250 - -


alloy steel plates with 1) 1)
austenitic stainless
steel cladding
For high service
temperatures
and/or certain
corrosive
conditions
3. FERROUS METALS - ALLOYED (CONT'd)

3.2 TUBES AND TUBING


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.2.1 Seamless 0.3 Mo +500 - 3059: Part 2 17175: A 49-213 - 2604-2 NOT for hydrogen
steel tubes - S2 243 15 Mo 3 TU 15 D 3 TS 26 service.
For boilers, super- 1) 1) 1) 1)
heaters and 1) Specify total
unfired heat 3606: Al content
transfer equip- CFS 243 0.012% max.
ment at high 1)
service
temperatures
3.2.2 Seamless 0.5 Mo +500 A 209 - T1 - - - G 3462 -
steel tubes 1) STBA 12
For boilers, super- Seamless
heaters and 1)
unfired heat
transfer equip-
ment at high
service
temperatures
3.2.3 Seamless 1 Cr-0.5 +600 A 213 - 3059: Part 2 17175: A 49-213 G 3462 2604-2 1) For resistance
Mo steel tubes T12 - S2 620-460 13 CrMo 4 TU 13 CD STBA 22 TS 32 to hydrogen
For boilers, 3) 4) 3) 4) 4 4-04 Seamless 3) 4) attack, see API
superheaters and 2) 3) 4) 2) 3) 4) 3) 4) 941.
unfired heat 3606:
transfer CFS 620 2) When
equipment at 3) 4) resistance to
high service hydrogen
temperatures attack is
and/or requiring required
resistance to specify
hydrogen attack Cr content
1) 0.8% min., see
API 941.
3.2.4 Seamless 1.25 Cr- +600 A 213 - - - A 49-213 G 3462 - 3) Specify to be
0.5 Mo steel tubes T11 TU 10 CD STBA 23 normalized and
For boilers, 3) 4) 5) 3606: 5-05 3) 4) 5) tempered or
superheaters and CFS 621 3) 4) 5) quenched and
unfired heat 3) 4) 5) tempered.
transfer
equipment at 4) See below.
high service
temperatures 5) Specify
and/or requiring P 0.005% max.
resistance to
hydrogen attack
1)
`4) Specify:
qCu 0.20% max.
Ni 0.30% max.
(%Si+%Mn)  1.10
(%Si+%Mn) x (%P+%Sn) x 104  150.
3. FERROUS METALS - ALLOYED (Cont'd)

3.2 TUBES AND TUBING (Cont'd)


DESIGNATION AND Metal ASTM BS DIN AFNOR JIS ISO REMARKS
APPLICATION Temp., °C
(See 1.7)
3.2.5 Seamless 2.25 Cr-1 +625 A 213 - 3059: Part 2 17175: A 49-213 G 3462 2604-2 1) For resistance to
Mo steel tubes T22 - S2 622-490 10 CrMo 9 TU 10 CD STBA 24 TS 34 hydrogen attack,
For boilers, 2) 3) 2) 3) 10 9-10 2) 3) 2) 3) see API 941.
furnaces, super- 2) 3) 2) 3)
heaters and 3606: 2) Specify to be
unfired heat CFS 622 normalized and
transfer 2) 3) tempered or
equipment at quenched and
high service tempered.
temperatures
requiring
optimum creep
resistance and/or
resistance to
hydrogen attack
1)
3.2.6 Seamless 5 Cr-0.5 +650 A 213 - T5 3606: - A 49-213 G 3462 2604-2 3) See below.
Mo steel tubes 2) CFS 625 TUZ 12 STBA 25 TS 37
For high service 2) CD 05-05 2) 2)
temperatures 2)
and/or resistance
to sulphur
corrosion, eg.
furnace tubes
3.2.7 Seamless 9 Cr-1 Mo +650 A 213 - T9 3059: - A 49-213 G 3462 2604-2
steel tubes 2) S2 629-470 TUZ 10 STBA 26 TS 38
For high service 2) CD 09 2) 2)
temperatures 2)
and/or resistance
to sulphur
corrosion, eg.
furnace tubes
3.2.8 Seamless 3.5 Ni steel (+400) - 3603: 17173: A 49-230 G 3464 2604-2 1) For low-
tubes 1) CFS 503 LT 10 Ni 14 TU 10 N STBL 450 TS 43 temperature
For low service Cat. 2 14 applications, see
temperatures Appendix 1 and
DEP 30.10.02.31-
Gen.
3.2.9 Seamless 9 Ni steel -200 - 3603: 17173: A 49-230 G 3464 2604-2
tubes 1) CFS 509 LT X 8 Ni 9 TUZ 6 N STBL 690 TS 45
Cat. 2 9
3.2.10 Seamless 12 Cr steel +540 A 268 - - 17456: - G 3463 - 1) TP 405 not to be
tubes TP 405 X 6 Cr Al SUS 405 used above
For unfired heat 1) 13 TB 400 °C.
transfer or 1) 1) 2) Composition in
equipment under A 268 - - - - accordance with
certain corrosive TP 410S - - ASTM A240 Type
conditions 2) 410S. All
requirements of
A268 shall be
fulfilled.
3.2.11 Seamless and welded (-200) A 269 - - - - - - 1) For tubes
18 Cr-10 N-2Mo steel +500 TP 316 intended for use
tubes 1) with compression
For certain or fittings, hardness
general A 269 - - - - - - shall not exceed
applications TP 316L 90 HRB
1)
3) Specify:
Cu 0.20% max.
Ni 0.30% max.
(%Si+%Mn)  1.10
(%Si+%Mn) x (%P+%Sn) x 104  150.
3. FERROUS METALS - ALLOYED (Cont'd)

3.2 TUBES AND TUBING (Cont'd)


DESIGNATION AND Metal ASTM BS DIN AFNOR JIS ISO REMARKS
APPLICATION Temp., °C
(See 1.7)
3.2.12 Welded 18 Cr-8 Ni -200 A 249 - 3605: 17457: - G 3463 2604 - 5 1) For low-temperature
steel tubes (+400) TP 304 LWHT X 5 CrNi SUS 304 TW 47 - applications, see
For superheaters 1) 2) 3) 304S31 18 10 TB LWHT Appendix 1 and DEP
and unfired heat 2) 3) or 2) 3) 2) 3) 4) 2) 3) 30.10.02.31-Gen.
transfer
equipment to 3606: 2) The tubes are welded
prevent product LWHT without the addition of
contamination or 304S31 filler metal, so the
for low service A 249 - 2) 3) 17457: - 2604-5 inside diam eter and
temperatures TP 304L X 2 CrNi G 3463 TW46- the wall thickness of
2) 3) 3605: 19 11 SUS 304 LWHT the tubes are
LWHT 2) 3) LTB 2) 3) restricted to DN100
304S11 2) 3) 4) max. and 5.5 mm
2) 3) or max., respectively. A
non-destructive
3606 electric test in
LWHT accordance with
304S11 ASTM A450 shall be
2) 3) carried out in addition
to the hydrostatic test.
3.2.13 Welded 18 Cr-8 Ni (-100) A 249 - 3605: 17457: - G 3463 2604-5
stabilized steel tubes +600 TP 321 LWHT X 6 CrNiTi - SUS 321 TW53- 3) The material shall be
For superheaters 2) 3) 321S31 18 10 TB LWHT capable of passing
and unfired heat 2) 3) or 2) 3) 2) 3) 4) 2) 3) the Practice E
transfer 3606 intergranular
equipment under LWHT corrosion test as
certain corrosive 321S31 specified in ASTM
conditions 2) 3) A262.
A 249 - 17457: 2604-5
TP 347 3605: X 6 CrNiNb G 3463 TW50-
2) 3) LWHT 18 10 SUS 347 LWHT
347S31 2) 3) TB 2) 3)
2) 3) or 2) 3) 4)
3606
LWHT
347S31
2) 3)
3.2.14 Welded 18 Cr-10 Ni-2 -200 A 249 - 3605: 17457: - G 3463 2604-5
Mo steel tubes +500 TP 316 LWHT X5 SUS 316 TW60- 4) Specify automatic
For superheaters 1) 2) 3) 316S31 CrNiMo 17 TB LWHT arc welded.
and unfired heat 2) 3) 12 2 2) 3) 4) 2) 3)
transfer or 2) 3)
equipment under 3606
certain corrosive LWHT
conditions 316S31
A 249 - 2) 3) 2604-5
TP 316L 17457: G 3463 TW57-
2) 3) 3605: X2 SUS 316L LWHT
LWHT CrNiMo - TB 2) 3)
316S11 17 13 2 2) 3) 4)
2) 3) 2) 3)
or
3606
LWHT
316S11
2) 3)
3.2.15 Welded 20 Cr-18 Ni-6 (-200) A 249 - - - - - -
Mo Cu-N steel tubes (+400) S 31254
For superheaters 2)
and unfired heat
transfer
equipment under
certain corrosive
conditions
3. FERROUS METALS - ALLOYED (Cont'd)

3.2 TUBES AND TUBING (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.2.16 Seamless 18 Cr-8 Ni -200 A 213 - 3606: 17458: A 49-217 G 3463 2604-2 1) For low-
steel tubes +400 TP 304 CFS 304S31 X 5 CrNi TUZ 6 SUS 304 TS47 temperature
For unfired heat 1) 2) 2) 18 10 CN 18 09 TB 2) applications,
transfer 2) 2) Seamless see Appendix 1
equipment to 2) and DEP
prevent product A 213 - 3606: 17458: A 49-217 2604-2 30.10.02.31-
contamination or TP 304L CFS 304S11 X 2 CrNi TUZ 2 G 3463 TS 46 Gen.
for low service 2) 2) 19 11 CN 18 10 SUS 304L 2)
temperatures 2) 2) TB
Seamless
2)
3.2.17 Seamless 18 Cr-8 Ni (-100) A 213 - - 17458: A 49-214 G 3463 2604-2 2) The material
stabilized steel tubes +600 TP 321 X 6 CrNiTi Z 6 CNT SUS 321 TS 53 shall be
For superheaters 2) 18 10 18 - 12B TB 2) capable of
and unfired heat 2) 2) Seamless passing the
transfer 2) Practice E
equipment under 3606: - A 49-217 intergranular
certain corrosive CFS 321S31 TUZ 6 corrosion test
conditions and/or 2) CNT 18 as specified in
at high service 10 ASTM A 262.
temperatures 2)

A 213 - - 17458: A 49 -214 2604-2


TP 347 X 6 CrNiNb Z 6 CNNb G 3463 TS 50
2) 18 10 18 - 12B SUS 347 2)
2) 2) TB
Seamless
3606: - 2)
CFS 347S31 -
2)
3.2.18 Seamless 18 Cr-8 Ni +815 A 213 - 3059: Part 2 - A 49-214 G 3463 2604-2 1) Specify
steel tubes TP 304H - CFS Z 6 CN SUS 304 TS 48 C 0.06% max.
For boilers, 1) 304S51 19-10 HTB 1) and Mo+Ti+Nb
superheaters and 1) 1) Seamless 0.4% max.
unfired heat 1)
transfer 2) The use of this
equipment at grade is subject
extreme service to agreement of
temperatures the Principal.
under certain
corrosive
conditions
3.2.19 Seamless 18 Cr-8 Ni +815 A 213 - 3059: Part 2 - - G 3463 2604-2
stabilized steel tubes TP 321H - CFS SUS 321 TS 54
For boilers, 2) 321S51 HTB 2)
superheaters and 2) Seamless
unfired heat 2)
transfer
equipment at A 213 - - - G 3463 2604-2
extreme service TP 347H 3059: Part 2 SUS 347 TS 56
temperatures 2) - CFS HTB 2)
under certain 347S51 Seamless
corrosive 2) 2)
conditions
3. FERROUS METALS - ALLOYED (Cont'd)

3.2 TUBES AND TUBING (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.2.20 Seamless 18 Cr-10 -200 A 213 - - 17458: A 49-214 G 3463 2604-2 1) For low-
Ni-2 Mo steel tubes +500 TP 316 X5 Z 6 CND SUS 316 TS60 temperature
For superheaters 1) 2) 3) CrNiMo 17 17-12B TB 2) 3) applications,
and unfired heat 12 2 2) 3) Seamless see Appendix 1
transfer 2) 3) 2) 3) and DEP
equipment under 3606: A 49-217 30.10.02.31-
certain corrosive CFS 316S31 TUZ 6 Gen.
conditions and/or 2) 3) CND 17 2) May be used
at high service 11 only for welded
temperatures 3) items with wall
A 213 - - 2604-2 thicknesses
TP 316L 17458: - G 3463 TS57 less than
3) X2 SUS 316 3) 10 mm and for
CrNiMo 17 LTB non-welded
3606: 13 2 Seamless items.
CFS 316S11 3) A 49-217 3) 3) The material
3) TUZ 2 shall be
CND 17 capable of
12 passing the
3) Practice E
intergranular
corrosion test
as specified in
ASTM A 262.
3.2.21 Seamless 18 Cr-8 Ni +815 A 271 - - - - G 3467 - 1) Wall thickness
steel tubes TP 321H SUS 321 max. 25 mm.
For furnaces 1) HTF
under certain 1)
corrosive -
conditions A 271 - - - - G 3467
TP 347H SUS 347
1) HTF
1)
3.2.22 Seamless 22 Cr-5 Ni- +300 A 789 - - - A 49-217 G 3463 - 1) Specify
Mo-N steel tubes S31803 TUZ2 SUS 329 seamless.
For certain 1) 2) CND 22 J2 LTB 2) N 0.15% min.
corrosive 05 03 2) 3) Mo 3.0% min.
conditions 2) 4) N 0.24% min.
3.2.23 Seamless 25 Cr-7 Ni- +300 A 789 - - - A 49-217 - -
Mo-N steel tubes S32750 TUZ2
For certain 1) CND 25
corrosive 07 03
conditions 3) 4)
3.2.24 Seamless 20 Cr- (-200) A 269 - - - A 49-217 - -
18 Ni-6 Mo-Cu-N (+400) S31254 TUZ1
steel tubes 1) CNDU 20
For certain 181 6 Az
corrosive
conditions
3. FERROUS METALS - ALLOYED (Cont'd)

3.3 PIPE
DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.3.1 Electric-fusion-welded +500 A 672 - - - - - - NOT for hydrogen
0.5 Mo steel pipe, L65 service
sizes larger than Class 32
DN400 1) 1) Specify total Al
For high service content
temperatures 0.012% max.

3.3.2 Electric-fusion-welded +600 A 691 - - - - - - 1) For resistance


1 Cr-0.5 Mo steel pipe 1 CR to hydrogen
in sizes DN400 and Class 22 attack, see API
larger or 42 941.
For high service 2) 3) 4)
temperatures,
requiring optimum
creep resistance
and/or resistance
to hydrogen
attack
1)
3.3.3 Electric-fusion-welded +600 A 691 - - - - - - 2) For Class 22,
1.25 Cr-0.5 Mo steel 1.25 CR base material
pipe in sizes DN400 Class 22 to be in
and larger or 42 N & T or Q & T
For high service 2) 3) 4) 5) condition, with
temperatures, tempering at
requiring optimum 730 °C min.
creep resistance Welds to be
and/or resistance PWHT in range
to hydrogen 680-780 °C.
attack
1)
3.3.4 Electric-fusion-welded +625 A 691 - - - - - - 3) For Class 42,
steel pipe in sizes 2.25 CR tempering
DN400 and larger Class 22 temperature to
For high service or 42 be 680 °C min.
temperatures, 2) 3) 4)
requiring optimum 4) See below.
creep resistance
and/or resistance 5) Specify
to hydrogen P 0.005% max.
attack
1)
3.3.5 Electric-fusion-welded +650 A 691 - - - - - -
5 Cr-0.5 Mo steel pipe 5 CR
in sizes DN400 and Class 22
larger or 42
For high service 2) 3)
temperatures
and/or resistance
to sulphur
corrosion
4) Specify:
Cu 0.20% max., Ni 0.30% max.
(%Si+%Mn)  1.10
(%Si+%Mn) x (%P+%Sn) x 104  150.
For weld metal, specify:
10P+5Sb+4Sn+As  1500, where values are in mg/Kg.
3. FERROUS METALS - ALLOYED (Cont'd)

3.3 PIPE (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.3.6 Electric-fusion-welded -200 A 358 - - - - - - 1) For low-
18 Cr-8 Ni steel pipe +400 Grade 304 temperature
in sizes above DN300 1) Class 1 applications,
For certain 2) see Appendix 1
corrosive and DEP
conditions and/or A 358 - 30.10.02.31-
high service Grade Gen.
temperatures 304L
Class 1
2)
3.3.7 Electric-fusion-welded (-100) A 358 - - - - - - 2) The material
18 Cr-8 Ni stabilized +600 Grade 321 shall be
steel pipe in sizes Class 1 capable of
above DN300 2) 3) passing the
For certain Practice E
corrosive A 358 - - - - - - intergranular
conditions and/or Grade 347 corrosion test
high service Class 1 as specified in
temperatures 2) 3) ASTM A 262

3.3.8 Electric-fusion-welded -200 A 358 - - - - - - 3) For optimum


18 Cr-10 Ni-2 Mo +500 Grade 316 resistance to
steel pipe in sizes 1) Class 1 intergranular
above DN300 2) 3) corrosion,
For certain specify a
corrosive A 358 - stabilization
conditions and/or Grade heat treatment
high service 316L at
temperatures Class 1 950 °C
2) 3) subsequent to
solution heat
treatment, as
detailed in
ASTM A358
Supplementary
Requirement
S5.

3.3.9 Electric-fusion-welded (-200) A 358 - - - - - - 1) Specify


18 Cr-8 Ni steel pipe (+500) Grade C 0.06% max.
in sizes above DN300 304L and Mo+Ti+Nb
For certain Class 1 0.04% max.
corrosive 1)
conditions and/or
high service
temperatures
3.3.10 Seamless 0.3 Mo +500 - - 17175: A 49-213 - 2604-2 NOT for hydrogen
steel pipe 15 Mo 3 TU 15 D3 TS 26 service.
For high service 1) 1) 1)
temperatures 1) Specify total
Al content
0.012% max.
3. FERROUS METALS - ALLOYED (Cont'd)

3.3 PIPE (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.3.11 Seamless 0.5 Mo +500 A 335 - P1 - - - G 3458 - NOT for hydrogen
steel pipe 1) STPA 12 service.
For high service 1)
temperatures Seamless usually
not obtainable in
sizes larger than
DN400. For larger
sizes use ASTM
A672-L65 Class 32
(3.3.1).

1) Specify total
Al content
0.012% max.

3.3.12 Seamless 1 Cr-0.5 +600 A 335 - 3604: 17175: A 49-213 G 3458 2604-2 Seamless usually
Mo steel pipe P12 HFS 620-440 13 CrMo 4 TU 13 CD STPA 22 TS 32 not obtainable in
For high service 3) 4) Cat. 2 4 4-04 3) 4) 3) 4) sizes larger than
temperatures 3) 4) 2) 3) 4) 2) 3) 4) DN400. For larger
and/or resistance sizes use
to hydrogen ASTM A691 - 1 CR-
attack Class 22 or 42 (see
1) 3.3.2).

1) For resistance
to hydrogen
attack, see API
941.
2) Where
resistance to
hydrogen attack
is required
specify Cr
content to be
0.8% min.
3) Specify to be
normalized and
tempered or
quenched and
tempered.
4) See below.

4) Specify:
Cu 0.20% max., Ni 0.30% max.
(%Si+%Mn)  1.10
(%Si+%Mn) x (%P+%Sn) x 104 150.
3. FERROUS METALS - ALLOYED (Cont'd)

3.3 PIPE (Cont'd)


DESIGNATION AND Metal ASTM BS DIN AFNOR JIS ISO REMARKS
APPLICATION Temp., °C
(See 1.7)
3.3.13 Seamless 1.25 Cr- +600 A 335 - 3604: - A 49-213 G 3458 - Seamless usually
0.5 Mo steel pipe P11 HFS 621 TU 10 CD STPA 23 not obtainable in
For high service 2) 3) 4) Cat. 2 5-05 2) 3) 4) sizes larger than
temperatures 2) 3) 4) 2) 3) 4) DN400. For larger
and/or resistance sizes use
to hydrogen ASTM A691 -
attack 1.25 CR-Class 22
1) or 42 (3.3.3).

1) For resistance
to hydrogen
attack, see API
941.
2) Specify to be
normalized and
tempered or
quenched and
tempered.
3) See below.
4) Specify
P 0.005% max.
3.3.14 Seamless 2.25 Cr- +625 A 335 - 3604: 17175: A 49-213 G 3458 2604-2 Seamless usually
1 Mo steel pipe P22 HFS 622 10 CrMo 9 TU 10 CD STPA 24 TS 34 not obtainable in
For high service 2) 3) Cat. 2 10 9-10 2) 3) 2) 3) sizes larger than
temperatures, 2) 3) 2) 3) 2) 3) DN400. For larger
requiring optimum sizes use
creep resistance ASTM A691 -
and/or resistance 2.25 CR-Class 22
to hydrogen or 42 (see 3.3.4).
attack
1) 1) For resistance
to hydrogen
attack, see API
941.
2) Specify to be
normalized and
tempered or
quenched and
tempered.
3) See below.

3.3.15 Seamless 5 Cr-0.5 +650 A 335 - P5 3604: - A 49-213 G 3458 2604-2 Seamless usually
Mo steel pipe 1) HFS 625 TUZ 12 STPA 25 TS 37 not obtainable in
For high service Cat. 2 CD 05-05 1) 1) sizes larger than
temperatures 1) 1) DN400. For larger
and/or resistance sizes use
to sulphur ASTM A691 - 5 CR-
corrosion Class 22 or 42 (see
3.3.5).

1) Specify to be
normalized and
tempered or
quenched and
tempered.

3) Specify:
Cu 0.20% max., Ni 0.30% max.
(%Si+%Mn)  1.10
(%Si+%Mn) x (%P+%Sn) x 104  150.
3. FERROUS METALS - ALLOYED (Cont'd)

3.3 PIPE (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.3.16 Seamless 9 Cr-1 Mo +650 A 335 - P9 3604: - A 49-213 G 3458 2604-2 1) Specify to be
steel pipe 1) HFS 629-470 TUZ 10 STPA 26 TS 38 normalized and
For high service 1) CD 09 1) 1) tempered or
temperatures 1) quenched and
and/or resistance tempered
to sulphur
corrosion
3.3.17 Seamless 3.5 Ni steel (+400) A 333 - 3603: 17173: A 49-230 G 3460 2604-2 1) For low-
pipe 1) Grade 3 HFS 503 LT 10 Ni 14 TU 10 N STPL 450 TS 43 temperature
For low service Seamless Cat. 2 14 applications,
temperatures see Appendix 1
and DEP
30.10.02.31-
Gen.
3.3.18 Seamless 9 Ni steel -200 A 333 - 3603: 17173: A 49-230 G 3460 2604-2 2) Specify
pipe 1) Grade 8 HFS 509 LT X 8 Ni 9 TUZ 6 N STPL 690 TS 45 C 0.10% max.
For low service Seamless Cat. 2 9 S 0.002% max.
temperatures P 0.005% max.
2)
3.3.19 Seamless and welded -200 A 312 - 3605: 17458/57: - G 3459 2604-2 1) For low-
18 Cr-8 Ni steel pipe +400 TP 304 CFS 304S31 X 5 CrNi SUS 304 TS 47 temperature
in sizes to DN300 incl. 1) 2) 4) and 18 10 TP 4) applications,
For low service LWHT 2) 4) 2) 3) 4) see Appendix 1
temperatures or to 304S31 2604-5 and DEP
prevent product 2) 4) TFW 47 - 30.10.02.31-
contamination LWHT Gen.
2) 4) 2) Welded pipe
may be used up
to and including
5.5 mm wall
thickness.
3.3.20 Seamless and welded -200 A 312 - 3605: 17458/57: - G 3459 2604-2 3) For welded
18 Cr- 8 Ni steel +400 TP 304L CFS 304S11 X 2 CrNi SUS 304 TS 46 pipe, specify
pipe in sizes to 1) 2) 4) and 19 11 LTP 4) automatic arc
DN300 incl. LWHT 2) 4) 2) 3) 4) welded.
For certain 304S11 2604-5 4) The materials
corrosive 2) 4) TFW 46 - shall be
conditions and/or LWHT capable of
high service 2) 4) passing the
temperatures Practice E
intergranular
corrosion test
as specified in
ASTM A 262
3.3.21 Seamless and welded (-100) A 312 - 3605: 17458/57: - G 3459 2604-2 5) For optimum
18 Cr-8 Ni steel +600 TP 321 CFS 321S31 X 6 CrNiTi SUS 321 TS 53 resistance to
pipe in sizes to 2) 4) 5) and 18 10 TP 4) 5) intergranular
DN300 incl. LWHT 2) 4) 5) 2) 3) 4) 5) corrosion,
For certain 321S31 2604-5 specify a
corrosive 2) 4) 5) TFW 53 - stabilization
conditions and/or LWHT heat treatment
high service 2) 4) 5) at 950 °C
temperatures subsequent to
A 312 - 17458/57: - 2604-2 solution heat
TP 347 3605: X 6 CrNiNb G 3459 TS 50 treatment, as
2) 4) 5) CFS 347S31 18 10 SUS 347 4) 5) detailed in
and 2) 4) 5) TP ASTM A358
LWHT 2) 3) 4) 5) 2604-5 Supplementary
347S31 TFW 50 - Requirement
2) 4) 5) LWHT S5.
2) 4) 5)
3. FERROUS METALS - ALLOYED (Cont'd)

3.3 PIPE (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.3.22 Seamless and welded +815 A 312 - 3605: - - G 3459 2604-2 1) For low-
18 Cr-8 Ni stabilized TP 321H CFS 321S51 SUS 321 TS 54 temperature
steel pipe in sizes to 2) 3) HTP 3) applications,
DN300 incl. 2) 3) 4) see Appendix 1
For certain A 312 - 3605: - - G 3459 2604-2 and DEP
corrosive TP 347H CFS 347S51 SUS 347 TS 56 30.10.02.31-
conditions and/or 2) 3) HTP 3) Gen.
extreme service 2) 3) 4) 2) Welded pipe
temperatures may be used up
to and including
5.5 mm.
3.3.23 Seamless and welded -200 A 312 - 3605: 17458/57: - G 3459 2604-2 3) The use of this
18 Cr-10 Ni- 2 Mo +500 TP 316 CFS 316S31 X5 SUS 316 TS 60 grade is subject
steel pipe in sizes to 1) 2) 5) and CrNiMo 17 TP 5) to agreement of
DN300 incl. LWHT 12 2 2) 4) 5) 2604-5 the Principal.
For certain 316S31 2) 5) TFW 60- 4) For welded
corrosive 2) 5) LWHT pipe, specify
conditions and/or 2) 5) automatic arc
high service A 312 - welded.
temperatures TP 316L 3605: - G 3459 2604-2 5) The materials
2) 5) CFS 316S11 17458/57: SUS 316 TS 57 shall be
and X2 LTP 5) capable of
LWHT CrNiMo 17 2) 4) 5) 2604-5 passing the
316S11 13 2 TFW 57- Practice E
2) 5) 2) 5) LWHT intergranular
2) 5) corrosion test
as specified in
ASTM A 262.
3.3.24 Seamless and welded +500 A 312 - 3605: - - G 3459 2604-2 1) Specify
18 Cr-8 Ni steel pipe (+815) TP 304H CFS 304S51 SUS 304 TS 48 C 0.06% max.
in sizes to DN300 incl. 1) 1) HTP 1) and Mo+Ti+Nb
For certain 1) 0.4% max.
corrosive
conditions and/or
high service
temperatures

3.3.25 Seamless and welded +300 A 790 - - - - G 3459 - 1) For low-


22 Cr-5 Ni-Mo-N steel 1) S 31803 SUS 329 temperature
pipe 2) 3) J2LTP applications,
For certain 2) 3) 4) see Appendix 1
corrosive and DEP
conditions 30.10.02.31-
Gen.
3.3.26 Seamless and welded +300 A 790 - - - - - - 2) Specify
25 Cr-7 Ni-Mo-N steel 1) S 32750 N 0.15% min.
pipe 2) 3) 3) Welded pipe
For certain may be used up
corrosive to and including
conditions 5.5 mm wall
thickness.
3.3.27 Seamless and welded -200 A 312 - - - - - - 4) For welded
20 Cr-18 Ni-6 Mo-Cu- (+400) S31254 pipe, specify
N steel pipe 1) 3) automatic arc
For certain welded.
corrosive
conditions
3. FERROUS METALS - ALLOYED (Cont'd)

3.4 FORGINGS, FLANGES AND FITTINGS


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.4.1 0.5 Mo steel butt- +500 A 234 - 1640: WP1 - - - - NOT for hydrogen
welding fittings WP1 or 1) service
For high service WP1W
temperatures 1) Sizes up to DN400
incl. shall be
seamless. Larger
sizes may be either
seamless or
welded.

1) Specify total
Al content
0.012% max.

3.4.2 1 Cr-0.5 Mo steel +600 A 234 - - - - - - Sizes up to DN400


butt-welding fittings WP12 incl. shall be
For high service Class 2 or seamless. Larger
temperatures WP12W sizes may be either
and/or resistance Class 2 seamless or
to hydrogen 2) 3) welded.
attack
1) 1) For resistance
to hydrogen
attack, see API
941.
3.4.3 1.25Cr-0.5Mo steel +600 A 234 - 1640: WP11 - - - - 2) Specify to be
butt-welding fittings WP11 2) 3) 4) normalized and
For high service Class 2 or tempered or
temperatures WP11W quenched and
and/or resistance Class 2 tempered.
to hydrogen 2) 3) 4)
attack
1)
3.4.4 2.25 Cr-1 Mo steel +625 A 234 - 1640: WP22 - - - - 3) See below.
butt-welding fittings WP22 2) 3)
For extrem e Class 3 or 4) Specify
service WP22W P 0.005% max.
temperatures Class 3
and/or resistance 2) 3)
to sulphur
corrosion
1)
3.4.5 5 Cr-0.5 Mo steel +650 A 234 - 1640: WP5 - - - - Sizes up to DN400
butt-welding fittings WP5 or 1) incl. shall be
For high service WP5W seamless. Larger
temperatures 1) sizes may be either
and/or resistance seamless or
to sulphur welded.
corrosion
1) Specify to be
normalized and
tempered or
quenched and
tempered.

3) Specify:
Cu 0.20% max., Ni 0.30% max.
(%Si+%Mn)  1.10
(%Si+%Mn) x (%P+%Sn) x 104  150.
For weld metal, specify:
10P+5Sb+4Sn+As  1500, where values are in mg/Kg.
3. FERROUS METALS - ALLOYED (Cont'd)

3.4 FORGINGS, FLANGES AND FITTINGS (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.4.6 3.5 Ni steel butt- (+400) A 420 - 1640: WPL3 - - - - Sizes up to DN400
welding fittings 1) WPL3 or 2) incl. shall be
For low service WPL3W seamless. Larger
temperatures 2) sizes may be either
seamless or
welded.

1) For low-
temperature
applications,
see Appendix 1
and DEP
30.10.02.31-
Gen.
2) Specify to be
normalized.

3.4.7 9 Ni steel butt-welding -200 A 420 - - - - - Sizes up to DN400


fittings 1) WPL8 or incl. shall be
For low service WPL8W seamless. Larger
temperatures 2) 3) sizes may be either
seamless or
welded.

1) For low-
temperature
applications,
see Appendix 1
and DEP
30.10.02.31-
Gen.
2) Specify to be
double-
normalized and
tempered or
quenched and
tempered.
3) Specify
C 0.10% max.
S 0.002% max.
P 0.005% max.
3.4.8 18 Cr-8 Ni steel butt- -200 A 403 - 1640: - - - - Sizes up to DN400
welding fittings +400 WP304 WP304 incl. shall be
For low service 1) -S/WX/WU 2) seamless. Larger
temperatures or 2) sizes may be either
to prevent product seamless or
contamination welded.

3.4.9 18 Cr-8 Ni steel butt- -200 A 403 - 1640: - - - - 1) For low-


welding fittings +400 WP304L WP304L temperature
For certain 1) -S/WX/WU 2) applications,
corrosive 2) see Appendix 1
conditions and/or and DEP
high service 30.10.02.31-
temperatures Gen.
2) The material
shall be
capable of
passing the
Practice E
intergranular
corrosion test
as specified in
ASTM A262.
3. FERROUS METALS - ALLOYED (Cont'd)

3.4 FORGINGS, FLANGES AND FITTINGS (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.4.10 18 Cr-8 Ni steel butt- +815 A 403 - - - - - - Sizes up to DN400
welding fittings WP304H incl. shall be
For certain -S/WX/WU seamless. Larger
corrosive 1) sizes may be either
conditions and/or seamless or
extreme service welded.
temperatures
1) Specify
C 0.06% max.
and Mo+Ti+Nb
0.4% max.
3.4.11 18 Cr-8 Ni stabilized (-100) A 403 - 1640: - - - - 2) The material
steel butt-welding +600 WP321 WP321 shall be
fittings -S/WX/WU 2) 3) capable of
For certain 2) 3) passing the
corrosive Practice E
conditions and/or A 403 - intergranular
extreme service WP347 1640: corrosion test
temperatures -S/WX/WU WP321 as specified in
2) 3) 2) 3) ASTM A262.
3) For optimum
resistance to
intergranular
corrosion,
specify a
stabilization
heat treatment
at
950 °C
subsequent
solution heat
treatment.

3.4.12 18 Cr-8 Ni stabilized +815 A 403 - - - - - - 1) The use of this


steel butt-welding WP321H grade is subject
fittings -S/WX/WU to agreement of
For certain 1) the Principal.
corrosive -
conditions and/or A 403 - - - - -
extreme service WP347H
temperatures -S/WX/WU
1)
3.4.13 18 Cr-10 Ni-2 Mo -200 A 403 - 1640: - - - - Sizes up to DN400
steel butt-welding +500 WP316 WP316 incl. shall be
fittings 1) -S/WX/WU 2) seamless. Larger
For certain 2) sizes may be either
corrosive seamless or
conditions and/or welded.
high service A 403 -
conditions WP316L 1640: - - - - 1) For low-
-S/WX/WU WP316L temperature
2) 2) applications,
see Appendix 1
and DEP
30.10.02.31-
Gen.
2) The material
shall be
capable of
passing the
Practice E
intergranular
corrosion test
as specified in
ASTM A262.
3. FERROUS METALS - ALLOYED (Cont'd)

3.4 FORGINGS, FLANGES AND FITTINGS (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.4.14 22 Cr-5 Ni-Mo-N steel +300 A 815 - - - - - - Sizes up to DN400
butt-welding fittings 1) S31803 incl. shall be
For certain Class WP- seamless. Larger
corrosive S or WP- sizes may be either
conditions WX seamless or
2) welded.

1) For low-
temperature
applications,
see Appendix 1
and DEP
30.10.02.31-
Gen.
2) N 0.15% min.

3.4.15 20 Cr-18 Ni-6 Mo-Cu- (-200) A 403 - - - - - - Sizes up to DN400


N steel butt-welding (+400) WPS31254 incl. shall be
fittings 1) -S/WX/WU seamless. Larger
For certain sizes may be either
corrosive seamless or
conditions welded.

1) For low-
temperature
applications,
see Appendix 1
and DEP
30.10.02.31-
Gen.

3.4.16 0.5 Mo steel forgings +500 A 182 - - - - G 3203 2604-1 NOT for hydrogen
For tube sheets, F1 SFVA F1 F28 or F29 service
flanges, fittings,
valves and other 1) Specify total
pressure-retaining Al content
parts at high 0.012% max.
service
temperatures
3.4.17 0.5 Mo steel forgings +500 A 336 - - - - G 3203 2604-1
For heavy parts, F1 SFVA F1 F29
e.g. drum 1) 1) 1)
forgings, for high
service
temperatures
3. FERROUS METALS - ALLOYED (Cont'da)

3.4 FORGINGS, FLANGES AND FITTINGS (Cont'd)


DESIGNATION AND Metal ASTM BS DIN AFNOR JIS ISO REMARKS
APPLICATION Temp., °C
(See 1.7)
3.4.18 1 Cr-0.5 Mo steel forgings +600 A 182 - 1503: 620- 17243: A 36-602 G 3203 2604-1 1) For resistance
For tube sheets, F12 440 13 CrMo 15 CD SFVA F32 to hydrogen
flanges, fittings, valves Class 2 2) 5) 44 4.05 F12 2) 5) attack, see API
and other pressure- 2) 5) 2) 3) 4) 5) 2) 4) 5)) 2) 5) 941.
retaining parts at high
service temperatures 2) Specify to be
and/or requiring normalized and
resistance to hydrogen tempered or
attack quenched and
1) tempered.
3.4.19 1 Cr-0.5 Mo steel forgings +600 A 336 - 1503: 620- 17243: A 36-602 G 3203 2604-1 3) When
For heavy parts, e.g. F12 440 13 CrMo 15 CD SFVA F32 resistance to
drum forgings, for high 2) 5) 2) 5) 44 4.05 F12 2) 5) hydrogen attack
service temperatures 2) 3) 4) 5) 2) 4) 5) 2) 5) is required,
and/or requiring specify
resistance to hydrogen Cr content to be
attack 0.8% min.
1)
4) Specify
0.45% Mo min.
for hydrogen
service.
3.4.20 1.25 Cr-0.5Mo steel +600 A 182 - 1503: 621- - - G 3203 -
forgings F11 460 SFVA 5) See below.
For tube sheets, 2) 5) 6) 2) 5) 6) F11A
flanges, fittings, valves 2) 5) 6) 6) Specify
and other pressure- P 0.005% max.
retaining parts at high
service temperatures
and/or requiring
resistance to hydrogen
attack
1)
3.4.21 1.25 Cr-0.5 Mo steel +600 A 336 - 1503: 621- - - G 3203 -
forgings F11 460 SFVA
For heavy parts, e.g. 2) 5) 6) 2) 5) 6) F11A
drum forgings, for high 2) 5) 6)
service temperatures
and/or requiring
resistance to hydrogen
attack
1)
3.4.22 2.25 Cr-1 Mo steel forgings +625 A 182 - 1503: 622- 17243: A 36-602 G 3203 2604-1
For tube sheets, F22 560 10 CrMo 9 10 CD SFVA F34
flanges, fittings, valves 2) 5) 2) 5) 10 9.10 F22B 2) 5))
and other pressure- 2) 5) 2) 5) 2) 5)
retaining parts at high
service temperatures
and/or requiring
resistance to hydrogen
attack
1)
3.4.23 2.25 Cr-1 Mo steel forgings +625 A 336 - 1503: 622- 17243: A 36-602 G 3203 2604-1
For heavy parts, e.g. F22 560 10 CrMo 9 10 CD SFVA F34
drum forgings, for high 2) 5) 2) 5) 10 9.10 F22B 2) 5)
service temperatures 2) 5) 2) 5) 2) 5)
and/or requiring
resistance to hydrogen
attack
1)
5) Specify:
Cu 0.20% max., Ni 0.30% max.
(%Si+%Mn)  1.10
(%Si+%Mn) x (%P+%Sn) x 104  150.
3. FERROUS METALS - ALLOYED (Cont'd)

3.4 FORGINGS, FLANGES AND FITTINGS (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.4.24 3 Cr-1 Mo steel +625 A 182 - - - A 36-602 G 3203 - 1) For resistance to
forgings F21 10 CD SFVA hydrogen attack,
For tube sheets, 2) 3) 12.10 F21B see API 941.
flanges, fittings, 2) 3) 2) 3)
valves and other 2) Specify to be
pressure-retaining normalized and
parts at high tempered or
service quenched and
temperatures, tempered.
requiring optimum
creep resistance 3) See below.
and/or requiring
resistance to
hydrogen attack
1)
3.4.25 5 Cr-0.5 Mo steel +650 A 182 - 1503: 625- - A 36-602 G 3203 2604-1
forgings F5 590 Z 10 CD SFVA F37
For tube sheets, 2) 2) 5.05 F5B 2)
flanges, fittings, 2) 2)
valves and other
pressure-retaining
parts at extreme
service
temperatures
and/or requiring
resistance to
sulphur corrosion

3.4.26 3.5 Ni steel forgings (+400) A 350 - 1503: 503- 17280: - G 3205 2604-1 1) For low-
For tube sheets, 1) LF 3 490 10 Ni 14 SFL 3 F44 temperature
flanges, fittings, applications, see
valves and other Appendix 1 and
pressure-retaining DEP
parts at low service 30.10.02.31-Gen.
temperatures

3.4.27 9 Ni steel forgings -200 A 522 - 1503: 509- 17280: - - 2604-1 2) Specify
For tube sheets, 1) Type I 690 X 8 Ni 9 F45 C 0.10% max.
flanges, fittings, 2) 2) 2) 2) Si 0.30% max.
valves and other P 0.002% max.
pressure-retaining S 0.005% max.
parts at low service
temperatures
3.4.28 12 Cr steel forgings +540 A 182 - 970: 17440: - G 3214 -
For certain F6a 410S21 X 10 Cr 13 SUS
corrosive conditions F410
3.4.29 12 Cr steel forgings +540 A 182 - 1503: 17440: - G 3214 -
For tube sheets, F6a 410S21 X 10 Cr 13 SUS
flanges, fittings, F410
valves and other
pressure-retaining
parts under certain
corrosive conditions
and/or at high
service
temperatures
5) Specify:
Cu 0.20% max., Ni 0.30% max.
(%Si+%Mn) 1.10
(%Si+%Mn) x (%P+%Sn) x 104  150.
3. FERROUS METALS - ALLOYED (Cont'd)

3.4 FORGINGS, FLANGES AND FITTINGS (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.4.30 18 Cr-8 Ni steel -200 A 182 - 970: 304S31 17440: A 36-607 G 3214 2604-1 1) For low-
forgings +400 F304 2) X 5 CrNi Z 6 CN SUS F49 temperature
For low service 1) 2) 18 10 18-09 F304 2) applications,
temperatures or 2) 2) 2) see Appendix 1
to prevent product and DEP
contamination 30.10.02.31-
Gen.

3.4.31 18 Cr-8 Ni steel -200 A 182 - 1503: 17440: A 36-607 G 3214 2604-1 2) The material
forgings +400 F304 304S31 X 5 CrNi Z 6 CN SUS F49 shall be
For tube sheets, 1) 2) 2) 18 10 18-09 F304 2) capable of
flanges, fittings, 2) 2) 2) passing the
valves and other Practice E
pressure-retaining intergranular
parts at low corrosion test
service as specified in
temperatures or ASTM A262.
to prevent product
contamination
3.4.32 18 Cr-8 Ni steel -200 A 182 - 970: 304S11 17440: A 36-607 G 3214 2604-1
forgings +500 F304L 2) X 2 CrNi Z 2 CN SUS F46
For certain 1) 2) 19 11 18-10 F304L 2)
corrosive 2) 2) 2)
conditions and/or
high service
temperatures
3.4.33 18 Cr-8 Ni steel -200 A 182 - 1503: 17440: A 36-607 G 3214 2604-1
forgings +500 F304L 304S11 X 2 CrNi Z 2 CN SUS F46
For tube sheets, 1) 2) 2) 19 11 18-10 F304L 2)
flanges, fittings, 2) 2) 2)
valves and other
pressure-retaining
parts under
certain corrosive
conditions and/or
at high service
temperatures
3.4.34 18 Cr-8 Ni steel +815 A 182 - 1503: - - G 3214 2604-1 1) Specify
forgings F304H 304S51 SUS F48 C 0.06% max.
For tube sheets, 1) 1) F304H 1) and Mo+Ti+Nb
flanges, fittings, 1) 0.4% max.
valves and other
pressure-retaining
parts under
certain corrosive
conditions and/or
at extreme
service
temperatures
3. FERROUS METALS - ALLOYED (Cont'd)

3.4 FORGINGS, FLANGES AND FITTINGS (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.4.35 18 Cr-8 Ni stabilized +600 A 182 - 1503: 17440: A 36-607 G 3214 2604-1 1) The material
steel forgings F321 321S31 X 6 CrNiTi Z 6 CNT SUS F55 shall be
For tube sheets, 1) 2) 1) 2) 18 10 18-10 F321 1) 2) capable of
flanges, fittings, 1) 2) 1) 2) 1) 2) passing the
valves and other Practice E
pressure-retaining A 182 - 1503: 17440: A 36-607 2604-1 intergranular
parts under F347 347S31 X 6 CrNiNb Z 6 CNNb G 3214 F52 corrosion test
certain corrosive 1) 2) 1) 2) 18 10 18-10 SUS 1) 2) as specified in
conditions and/or 1) 2) 1) 2) F347 ASTM A262.
at high service 1) 2) 2) For optimum
temperatures resistance to
intergranular
corrosion,
specify a
stabilization
heat treatment
at
950 °C,
subsequent to
solution heat
treatment.

3.4.36 18 Cr-8 Ni stabilized +815 A 182 - 1503: - - G 3214 2604-1 1) The use of this
steel forgings F321H 321S51-490 SUS F54A grade is subject
For tube sheets, 1) 1) F321H 1) to agreement of
flanges, fittings, 1) the Principal.
valves and other
pressure-retaining A 182 - 1503: - - G 3214 2604-1
parts under F347H 347S51 SUS F51
certain corrosive 1) 1) F347H 1)
conditions and/or 1)
at extreme
service
temperatures
3.4.37 18 Cr-10 Ni-2 Mo -200 A 182 - 970: 316S31 17440: A 36-607 G 3214 2604-1 1) For low-
steel forgings +500 F316 2) X5 Z 6 CND SUS F62 temperature
For certain 1) 2) CrNiMo 17 17-11 F316 2) applications,
corrosive 12 2 2) 2) see Appendix 1
conditions and/or 2) and DEP
high service 30.10.02.31-
temperatures Gen.
3.4.38 18 Cr-10 Ni-2 Mo -200 A 182 - 1503: 17440: A 36-607 G 3214 2604-1 2) The material
steel forgings +500 F316 316S31 X5 Z 6 CND SUS F62 shall be
For tube sheets, 1) 2) 2) CrNiMo 17 17-11 F316 2) capable of
flanges, fittings, 12 2 2) 2) passing the
valves and other 2) Practice E
pressure-retaining intergranular
parts under corrosion test
certain corrosive as specified in
conditions and/or ASTM A262.
at high service
temperatures
3.4.39 18 Cr-10 Ni-2 Mo -200 A 182 - 970: 316S11 17440: A 36-607 G 3214 2604-1
steel forgings +500 F316L 2) X2 Z 2 CND SUS F59
For certain 1) 2) CrNiMo 17 17-11 F316L 2)
corrosive 13 2 2) 2)
conditions and/or 2)
high service
temperatures
3. FERROUS METALS - ALLOYED (Cont'd)

3.4 FORGINGS, FLANGES AND FITTINGS (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.4.40 18 Cr-10 Ni-2 Mo -200 A 182 - 1503: 17440: A 36-607 G 3214 2604-1 1) For low-
steel forgings +500 F316L 316S11 X2 Z 2 CND SUS F59 temperature
For tube sheets, 1) 2) 2) CrNiMo 17 17-11 F316L 2) applications,
flanges, fittings, 13 2 2) 2) see Appendix 1
valves and other 2) and DEP
pressure-retaining 30.10.02.31-
parts under Gen.
certain corrosive
conditions and/or
at high service
temperatures
3.4.41 22 Cr-5 Ni- Mo-N (-30) A 182 - 1503: SEW 400: - - - 2) The material
steel forgings +300 F51 318 S13 X2 shall be
For tube sheets, 1) 3) 3) CrNiMo capable of
flanges, fittings, N 22 5 3 passing the
valves and other 3) Practice E
pressure-retaining intergranular
parts under corrosion test
certain corrosive as specified in
conditions. ASTM A262.
3.4.42 25 Cr-7 Ni-Mo-N steel (-30) A 182 - - - - - - 3) N 0.15% min.
forgings +300 F53
For tube sheets, 1)
flanges, fittings,
valves and other
pressure-retaining
parts under
certain corrosive
conditions.
3.4.43 20 Cr-18 Ni-6 Mo-Cu- (-200) A 182 - - - - - -
N steel forgings (+400) F44
For tube sheets, 1)
flanges, fittings,
valves and other
pressure-retaining
parts under
certain corrosive
conditions.
3. FERROUS METALS - ALLOYED (Cont'd)

3.5 CASTINGS
DESIGNATION AND Metal ASTM BS DIN AFNOR JIS ISO REMARKS
APPLICATION Temp., °C
(See 1.7)
3.5.1 14.5 Si iron castings +250 A 518 - 1 1591: Si14 - - - - 1) Si content
For non-pressure- 1) 1) 14.5% min.
retaining (internal) Other alloying
parts in acid elements,
service e.g. Mo, may be
added.
3.5.2 15 Ni-6 Cu-2 Cr-Fe +500 A 436 - 3468: F1 1694: GGL A 32-301 - 2892:
(Ni-Resist Type 1) iron Type 1 NiCuCr 15 6 L-NUC L-NiCuCr
castings 2 15 6 2 15 6 2
For non-pressure-
retaining (internal)
parts under certain
corrosive
conditions
3.5.3 20 Ni-2 Cr ductile iron +500 A 439: 3468: S2 1694: GGG A 32-301 - 2892:
(Ni-Resist Type D-2) Type D-2 NiCr 20 2 S-NC 20 S-NiCr 20
castings 2 2
For pressure-
retaining parts
under certain
corrosive
conditions
3.5.4 22 Ni-4 Mn ductile iron -105 A 571: 3468: S2M 1694: GGG A 32-301 - 2892: 1) For low-
(Ni-Resist Type D-2M) +500 Type D-2M NiMn 23 4 S-NM 23 S-NiMn 23 temperature
castings 1) 4 4 applications,
For pressure- see Appendix 1
retaining parts at and DEP
low service 30.10.02.31-
temperatures Gen.
3.5.5 0.5 Mo steel castings +500 A 217 - 1504: 245 - A 32-055 G 5151 - NOT for hydrogen
For fittings, valves WC1 1) 20 D5-M SCPH 11 service
and other 1) 1) 2) 1)
pressure-retaining 1) Specify total
parts at high Al content
service 0.012% max.
temperatures 2) Specify
0.45% Mo min.
for hydrogen
service.
3.5.6 1.25 Cr-0.5 Mo steel +600 A 217 - 1504: 621 17245: A 32-055 G 5151 - 1) For resistance
castings WC6 2) 3) GS-17 CrMo 15 SCPH 21 to hydrogen
For fittings, valves 2) 3) 55 CD5.05-M 2) 3) attack, see API
and other 2) 3) 2) 3) 941.
pressure-retaining
parts at high 2) Specify to be
service normalized and
temperatures tempered or
and/or requiring quenched and
resistance to tempered.
hydrogen attack
1)
3.5.7 2.25 Cr-1 Mo steel +625 A 217 - 1504: 622 17245: A 32-055 G 5151 - 3) Specify
castings WC9 2) GS-18 CrMo 15 SCPH 32 P 0.005% max.
For fittings, valves 2) 9 10 CD9.10-M 2)
and other 2) 2)
pressure-retaining
parts at extreme
service
temperatures
requiring optimum
creep resistance
and/or resistance
to hydrogen attack
1)
3. FERROUS METALS - ALLOYED (Cont'd)

3.5 CASTINGS (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.5.8 5 Cr-0.5 Mo steel +650 A 217 - 1504: 625 SEW 595: A 32-055 G 5151 - 1) For resistance
castings C5 1) GS-12 Z 15 SCPH 61 to hydrogen
For fittings, valves 1) CrMo 19 5 CD5.05-M 1) attack, see API
and other pressure- 1) 1) 941.
retaining parts at
high service
temperatures and/or
requiring resistance
to sulphur corrosion
3.5.9 9 Cr-1 Mo steel castings +650 A 217 - 1504: 629 SEW 595: - -
For fittings, valves C12 1) G-X 12
and other pressure- 1) CrMo 10 1
retaining parts at 1)
high service
temperatures and/or
requiring resistance
to sulphur corrosion
3.5.10 3.5 Ni steel castings (+400) A 352 - 1504: SEW 685: A 32-053 G 5152 - 1) For low-
For low service 1) LC3 503LT60 GS-10 Ni FC 3-M SCPL 31 temperature
temperatures 14 or applications,
A 32-055 see Appendix 1
20 N 12- and DEP
M 30.10.02.31-
Gen.
3.5.11 9 Ni steel castings (+400) A 352 - - - - - - 2) Specify
For low service 1) LC9 C 0.10% max.
temperatures 2) S 0.002% max.
P 0.005% max.
3.5.12 12 Cr steel castings +540 A 743 - 3100: 17445: A 32-059 G 5121 -
For non-pressure- CA15 410C21 G-X 20 Z 12 C SCS1
retaining parts under Cr 14 13-M
certain corrosive
conditions
3.5.13 12 Cr steel castings +540 A 217 - 1504: 17445: A 32-059 G 5121 -
For pressure- CA15 420C29 G-X 20 Z 12 C SCS1
retaining parts Cr 14 13-M
under certain
corrosive conditions
3.5.14 18 Cr-8 Ni steel castings -200 A 744 - 3100: 17445: A 32-056 G 5121 - 1) For low-
For non-pressure- +400 CF8 304C15 G-X 6 Z 6 CN SCS13A temperature
retaining (internal) 1) 2) 2) CrNi 18 9 18-10-M 2) applications,
parts under certain 2) 2) see Appendix 1
corrosive conditions and DEP
and/or at high 30.10.02.31-
service temperatures Gen.
2) Castings for
corrosive
service shall be
capable of
meeting the
requirements of
ASTM A262,
Practice E.
3.5.15 18 Cr-10 Ni-Nb (-100) A 744 - 3100: 17445: A 32-056 G 5121 - 3) If intended for
stabilized steel castings +600 CF8C 347C17 G-X 5 Z 6 CNNb SCS21 working
For non-pressure- 2) 3) 2) 3) CrNiNb 18-10-M 2) 3) temperatures
retaining (internal) 18 9 2) 3) above 500 °C,
parts under certain 2) 3) specify Si
corrosive conditions content
and/or at high 1.0% max.
service temperatures
3. FERROUS METALS - ALLOYED (Cont'd)

3.5 CASTINGS (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.5.16 18 Cr-10 Ni-2 Mo steel -200 A 744 - 3100: 17445: A 32-056 G 5121 - 1) For low-
castings +500 CF8M 316C16 G-X 6 Z 6 CND SCS14A temperature
For non-pressure- 1) 2) 2) CrNiMo 18-12-M 2) applications,
retaining (internal) 18 10 2) see Appendix 1
parts under certain 2) and DEP
corrosive conditions 30.10.02.31-
and/or at high service Gen.
temperatures
2) Castings for
corrosive
service shall be
capable of
meeting the
requirements of
ASTM A262,
Practice E.
3.5.17 25 Cr-20 Ni steel castings +1000 A 297 - 3100: 17465: A 32-057 G 5122 - 3) If intended for
For non-pressure- HK 310C45 G-X 40 Z 40 CN SCH22 working
retaining (internal) 4) 4) CrNiSi 25.20-M 4) temperatures
parts requiring heat 25 20 4) above 500 °C,
resistance 4) specify Si
content
1.0% max.
3.5.18 25 Cr-12 Ni steel castings +1000 A 447 - 3100: - - G 5122 - 4) See DEP
For furnace tube Type II 309C32 SCH13A 31.24.40.31-
supports 4) 4) 5) 4) Gen.

3.5.19 18 Cr-8 Ni steel castings -200 A 351 - 1504: 17445: A 32-056 G 5121 -
For pressure-retaining +500 CF8 304C15 G-X 6 Z 6 CN SCS13A 5) Specify
parts under certain 1) 2) 2) CrNi 18 9 18-10-M 2) magnetic
corrosive conditions 2) 2) permeability
and/or at high service 1.05 max.
temperatures
3.5.20 18 Cr-8 Ni-Nb stabilized (-100) A 351 - 1504: 17445: A 32-056 G 5121 -
steel castings +600 CF8C 347C17 G-X 5 Z 6 CNNb SCS21
For pressure-retaining 2) 3) 2) 3) CrNiNb 18-10-M 2) 3)
parts under certain 18 9 2) 3)
corrosive conditions 2) 3)
and/or at high service
temperatures
3.5.21 18 Cr-10 Ni-2 Mo steel -200 A 351 - 1504: 17445: A 32-056 G 5121 -
castings +500 CF8M 316C16 G-X 6 Z 6 CND SCS14A
For pressure-retaining 1) 2) 2) CrNiMo 18-12-M 2)
parts under certain 18 10 2)
corrosive conditions 2)
and/or at high service
temperatures

3.5.22 22 Cr-5 Ni-Mo-N steel +300 A 890 - - - - - -


castings 4A, S32 &
For pressure-retaining S33
parts under certain
corrosive conditions
3.5.23 25 Cr-7 Ni-Mo-N steel +300 A 890 - - - - - -
castings 5A, S32 &
For pressure-retaining S33
parts under certain
corrosive conditions
3. FERROUS METALS - ALLOYED (Cont'd)

3.5 CASTINGS (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.5.24 20 Cr-18 Ni-6 Mo-Cu- (-200) A 351 - - - - - -
N steel castings (+400) CK3MCuN
For pressure-
retaining parts
under certain
corrosive
conditions
3.5.25 25 Cr-12 Ni steel +1000 A 351 - - - - G 5121 - 1) See DEP
castings CH20 SCS17 31.24.40.31-
For pressure- 1) 1) Gen.
retaining parts
under certain
corrosive
conditions at
extreme service
temperatures
3.5.26 25 Cr-20 Ni steel +1000 A 351 - - - - G 5121 -
castings CK20 SCS18
For pressure- 1) 1)
retaining parts
under certain
corrosive
conditions at
extreme service
temperatures
3.5.27 25 Cr-20 Ni steel +1000 A 351 - 1504: SEW: A 32-057 G 5122 - 1) See DEP
castings HK40 310C40 G-X 40 Z 40 CN SCH22 31.24.40.31-
For pressure- 1) 1) CrNiSi 25.20-M 1) Gen.
retaining parts 25 20 1)
under certain 1)
corrosive
conditions at
extreme service
temperatures
3.5.28 20 Cr- 29 Ni-Mo-Cu (+400) A 744 - 1504: - - G 5121 -
steel castings CN7M 332C11 SCS23
For fittings, valves
and other
pressure-retaining
parts requiring
resistance to
sulphuric acid
corrosion

3.5.29 Cr-Ni steel centrifugal 1) 1) - - - - - 1) See DEP


and static castings 31.24.40.31-
20 Cr-33 Ni-Nb Gen.
25 Cr-20 Ni
25 Cr-35 Ni-Nb
For pressure-
retaining furnace
parts at extreme
service
temperatures
3. FERROUS METALS - ALLOYED (Cont'd)

3.6 BARS, SECTIONS AND WIRE


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.6.1 1 Cr-0.25 Mo steel bars +450 A 322 - 970: 17200: A 35-552 G 4105 683-1
For machined parts (+540) 4140 708A40 42 CrMo 42 CD 4 SCM 440 42 CrMo
4 4
3.6.2 9 Ni steel bars -200 - 1502: 17280: - - - 1) For low-
For machined parts for 1) 509-650 X 8 Ni 9 temperature
low-temperature 2) applications, see
service Appendix 1 and
- 1502: 17280: - - - DEP 30.10.02.31-
509-690 X 8 Ni 9 Gen.
4) 3) 4) 2) Double normalized
and tempered
condition.
3) Quenched and
tempered
condition.
4) Specify
C 0.10% max.
S 0.002% max.
P 0.005% max.
3.6.3 12 Cr steel bars +425 A 276 - 970: 17440: A 35-574 G 4303 683-13 1) Free-machining
For machined parts Type 410 410S21 X 15 Cr Z 10 C 13 SUS 410 Type 1 quality ASTM
1) 13 A582 Type 416 or
416Se acceptable,
subject to approval
A 276 - 970: A 35-574 G 4303 by the Principal.
Type 420 420S37 17440: Z 20 C 13 SUS For welded items
1) X 20 Cr 420J2 specify Type 405.
13
3.6.4 18 Cr-8 Ni steel bars -200 A 479 - 970: 17440: A 35-574 G 4303 683-13 1) For low-
For machined parts +500 Type 304 304S31 X 5 CrNi Z 6 CN SUS 304 Type 11 temperature
1) 2) 2) 18 10 18-09 2) 2) applications, see
2) 2) Appendix 1 and
DEP 30.10.02.31-
Gen.
3.6.5 18 Cr-8 Ni steel bars -200 A 479 - 970: 17440: A 35-574 G 4303 683-13 2) The material shall
For machined parts +500 Type 304S11 X 2 CrNi Z 2 CN SUS 304L Type 10 be capable of
1) 304L 2) 19 11 18-10 2) 2) meeting the
2) 2) 2) requirements of
ASTM A262
Practice E.
3.6.6 18 Cr-8 Ni steel bars +500 A 479 - - - - - - 1) Specify
For machined parts (+815) Type C 0.06% max.
304H and Mo+Ti+Nb
1) 0.4% max.
3.6.7 18 Cr-8 Ni stabilized steel (-200) A 479 - 970: 17440: A 35-574 G 4303 683-13 1) For low-
bars +815 Type 321 321S31 X 6 CrNiTi Z 6 CNT SUS 321 Type 15 temperature
For machined parts 2) 2) 18 10 18-10 2) 2) applications, see
2) 2) Appendix 1 and
DEP 30.10.02.31-
A 479 - 970: 17440: - G 4303 683-13 Gen.
Type 347 347S31 X 6 CrNiN SUS 347 Type 16 2) The material shall
2) 2) b 18 10 2) 2) be capable of
2) meeting the
requirements of
ASTM A262
Practice E.
3. FERROUS METALS - ALLOYED (Cont'd)

3.6 BARS, SECTIONS AND WIRE (CONT'D)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.6.8 18 Cr-8 Ni stabilized +500 A 479 - - - - - - 1) The use of this
steel bars (+815) Type 321H grade is subject
For machined 1) to agreement of
parts the Principal
- - - - -
A 479 -
Type 347H
1)
3.6.9 18 Cr-10 Ni-2 Mo -200 A 479 - 970: 316S31 17440: A 35-574 G 4303 683-13 1) For low-
steel bars +500 Type 316 2) X 5 CrNiM Z 7 CND SUS 316 Type 20 temperature
For machined 1) 2) o 17 12 2 17-11-02 2) 2) applications,
parts 2) 2) see Appendix 1
and DEP
30.10.02.31-
Gen.
3.6.10 18 Cr-10 Ni-2 Mo -200 A 479 - 970: 316S11 17440: A 35-574 G 4303 683-13 2) The material
steel bars +500 Type 316L 2) X 2 CrNiM Z 3 CND SUS 316L Type 19 shall be
For machined 1) 2) o 17 13 2 17-11-02 2) 2) capable of
parts 2) meeting the
requirements of
ASTM A262
Practice E.

3.6.11 22 Cr-5 Ni-Mo-N steel -30 A 479 - - - - - - 1) For low-


bars +300 S31803 temperature
For machined 1) 2) applications,
parts see Appendix 1
and
DEP
3.6.12 25 Cr-7 Ni-Mo-N steel -30 A 479 - - - - - - 30.10.02.31-
bars +300 S32750 Gen.
For machined 1)
parts 2) N 0.15% min.
3.6.13 20 Cr-18 Ni-6 Mo-Cu- (-200) A 276 - - - - - - 1) For low-
N steel bars (+400) S31254 temperature
For machined 1) applications,
parts see Appendix 1
and DEP
30.10.02.31-
Gen.

3.6.14 Si-Mn steel bars +230 A 689/A 970: 251A60 - A 35-571 G 4801 -
For springs 322-9260 61 SC 7 SUP 7
3.6.15 Cold drawn steel wire (+230) A 227 5216 17223 - G 3521 -
For springs
3.6.16 Cold drawn 18 Cr-8Ni -200 A 313 - 2056: 17224: A 35-574 G 4314 - 1) For low-
steel wire +230 Type 302 302S26 X 12 CrNi Z 12 SUS 302 temperature
For springs 1) 2) 2) 17 7 CN 18-09 2) applications,
2) 2) see Appendix 1
and DEP
30.10.02.31-
Gen.
2) The material
shall be
capable of
meeting the
requirements of
ASTM A262
Practice E.
3. FERROUS METALS - ALLOYED (Cont'd)

3.7 BOLTING
DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.7.1 1 Cr-0.25 Mo steel bolting +450 A 193 - B7 4882: B7 17200: A 35-557 G 4107 683-1 For nuts see 2.7.3.
material (+540) 42 CrMo 4 42 CD 4 SNB7 42 CrMo 4
For general use (Q+T)
3.7.2 1 Cr-0.25 Mo steel bolting +450 A 193 - 4882: B7M - - - - For nuts see 3.7.13.
material (+540) B7M
For sour service
3.7.3 1 Cr-0.5 Mo-0.25 V steel +525 A 193 - 4882: B16 17240: A 35-558 G 4107 - For nuts see 3.7.14.
bolting material (+600) B16 40 CrMoV 42 CDV 4 SNB16
For high-temperature 47
service
3.7.4 1 Cr-0.25 Mo steel bolting -105 A 320 - L7 4882: L7 - - - - 1) For low-
material +450 temperature
For low-temperature (+540) applications,
service 1) see Appendix 1
and DEP
30.10.02.31-
Gen.

For nuts see 3.7.15.

3.7.5 1 Cr-0.25 Mo steel bolting -30 A 320 - 4882: L7M - - - - 1) For low-
material +450 L7M temperature
For sour service and 1) applications,
low-temperature see Appendix 1
service and DEP
30.10.02.31-
Gen.

For nuts see 3.7.16.

3.7.6 9 Ni steel bolting material -200 - 4882: L9 - - - - 1) For low-


For low-temperature 1) temperature
service applications,
- 4882: L9A - - - - see Appendix 1
and DEP
30.10.02.31-
Gen.

For nuts see 3.7.17.

3.7.7 12 Cr steel bolting material +425 A 193 - 4882: B6 17440: A 35-574 G 4303 - For nuts see 3.7.18.
For certain corrosive (+540) B6X X 20 Cr 13 Z 20 C 13 SUS
conditions 420J2
3.7.8 18 Cr-8 Ni steel (strain -200 A 193 - B8 4882: B8X 17440: A 35-574 G 4303 - 1) For low-
hardened) bolting material +815 Class 2 2) X 5 CrNi Z 6 CN SUS temperature
For certain corrosive 1) 2) 18 10 18-09 304 applications,
conditions and/or 2) 2) 2) see Appendix 1
extreme-temperature and DEP
service 30.10.02.31-
Gen.
2) The material
shall be
capable of
meeting the
requirements of
ASTM A262
Practice E.

For nuts see 3.7.19.


3. FERROUS METALS - ALLOYED (Cont'd)

3.7 BOLTING (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.7.9 18 Cr-8 Ni stabilized -200 A 193 - 4882: B8T 17440: A 35-574 G 4303 - 1) For low-
steel bolting material +815 B8T 2) X 6 CrNiTi Z 6 CNT SUS 321 temperature
For certain 1) 2) 18 10 18-10 2) applications,
corrosive 2) 2) see Appendix 1
conditions and/or and DEP
extreme- 4882: B8C 17440: - G 4303 30.10.02.31-
temperature A 193 - 2) X 6 CrNiNb SUS 347 Gen.
service B8C 18 10 2) 2) The material
2) 2) shall be
capable of
meeting the
requirements of
ASTM A262
Practice E.

For nuts see 3.7.21.

3.7.10 18 Cr-10 Ni-2 Mo -200 A 193 - 4882: B8MX 17440: A 35-574 G 4303 - 1) For low-
steel (strain +500 B8M 2) X5 Z 7 CND SUS 316 temperature
hardened) bolting 1) Class 2 CrNiMo 17 17-11-02 2) applications,
material 2) 12 2 2) see Appendix 1
For certain 2) and DEP
corrosive 30.10.02.31-
conditions and/or Gen.
high-temperature 2) The material
service shall be
capable of
meeting the
requirements of
ASTM A262
Practice E.

For nuts see 3.7.22.

3.7.11 18 Cr-8 Ni steel -200 A 193 - 4882: B8N - - G 4303 - 1) For low-
bolting material 1) B8N 2) SUS 304 temperature
For low- 2) N1 applications,
temperature 2) see Appendix 1
service and DEP
30.10.02.31-
Gen.
2) The material
shall be
capable of
meeting the
requirements of
ASTM A262
Practice E.

For nuts see 3.7.20.

3.7.12 Precipitation harden- (+540) A 453-660 4882: B17B - A 35-574 G 4311 - For nuts see 3.7.23.
ing austenitic Ni-Cr Class A Z6 SUH 660
steel bolting material NCTDV
For certain 25-15 B
corrosive
conditions and/or
high-temperature
service.
Expansion
coefficient
comparable with
austenitic steels
3. FERROUS METALS - ALLOYED (Cont'd)

3.7 BOLTING (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.7.13 0.25 Mo steel nuts +525 A 194 - 4882: 2HM - - - -
For bolting made 2HM
from material
specified under
3.7.2
3.7.14 0.25 Mo steel nuts +525 A 194 - 4 4882: 4 - A 35-557 - -
For bolting made (600) 42 CD 4
from material
specified under
3.7.3
3.7.15 0.25 Mo steel nuts -105 A 194 - 4882: L4 - - - - 1) For low-
For bolting made +525 4,S4 temperature
from material (+600) applications,
specified under 1) see Appendix 1
3.7.4 and DEP
30.10.02.31-
Gen.

3.7.16 0.25 Mo steel nuts +525 A 194 - 4882: L7M - - - - 1) For low-
For bolting made 7M,S4 temperature
from material applications,
specified under see Appendix 1
3.7.5 and DEP
30.10.02.31-
Gen.

3.7.17 9 Ni steel nuts -200 - 4882: L9 - - - - 1) For low-


For bolting made 1) temperature
from material - 4882: L9A - - - - applications,
specified under see Appendix 1
3.7.6 and DEP
30.10.02.31-
Gen.

3.7.18 12 Cr steel nuts +425 A 194 - 6 4882: 6 17440: A 35-574 G 4303 - 1) Free-machining
For bolting made (+540) 1) X 20 Cr 13 Z 20 C 13 SUS Grade 6F
from material 420J2 acceptable,
specified under subject to
3.7.7 approval of the
Principal.

3.7.19 18 Cr-8 Ni steel -200 A 194 - 4882: 8X 17440: A 35-574 G 4303 - 1) For low-
(strain hardened) nuts +815 8,S1 3) X 5 CrNi Z 6 CN SUS 304 temperature
For bolting made 1) 2) 3) 18 10 18-09 3) applications,
from material 3) 3) see Appendix 1
specified under and DEP
3.7.8 30.10.02.31-
Gen.
3.7.20 18 Cr-8 Ni steel nuts -200 A 194 - 8N 4882: 8N - - - - 2) Free-machining
For low- 1) 3) 3) Grade 8F
temperature acceptable,
service. subject to
For bolting made approval of the
from material Principal.
specified under 3) The material
3.7.11. shall be
capable of
meeting the
requirements of
ASTM A262
Practice E.
3. FERROUS METALS - ALLOYED (Cont'd)

3.7 BOLTING (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
3.7.21 18 Cr-8 Ni stabilized -200 A 194 - 8T 4882: 8T 17440: A 35-574 G 4303 - 1) For low-
steel nuts +815 2) 3) 3) X 6 CrNiTi Z 6 CNT SUS 321 temperature
For bolting made 1) 18 10 18-10 3) applications,
from material 3) 3) see Appendix 1
specified under and DEP
3.7.9 A 194 - 8C 4882: 8C 17440: - G 4303 - 30.10.02.31-
2) 3) 3) X 6 CrNiNb SUS 347 Gen.
18 10 3) 2) Free-machining
3) Grade 8F
acceptable,
subject to
approval of the
Principal.
3.7.22 18 Cr-10 Ni-2 Mo -200 A 194 - 4882: 8MX 17440: A 35-574 G 4303 - 3) The material
steel (strain +500 8M,S1 3) X5 Z 7 CND SUS 316 shall be
hardened) nuts 1) 3) CrNiMo 17-11-02 3) capable of
For bolting made 17 12 2 3) meeting the
from material 3) requirements of
specified under ASTM A262
3.7.10 Practice E.

3.7.23 Precipitation harden- (+540) A 453-660 4882: B17B - A 35-574 G 4311 -


ing austenitic Ni-Cr Class A Z6 SUH 660
steel nuts NCTDV
For bolting made 25-15 B
from material
specified under
3.7.12
4. NON-FERROUS METALS

4.1 PLATES, SHEETS AND STRIP


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.1.1 Aluminium plates and - 200 B 209 - 1470: 1050A 1745: A 50-451 H 4000 209-1/2 Specify annealed
sheets +200 Alloy 1060 1) Al99.5 1050 A A 1050 P Al99.5 condition for all
For certain corrosive grades.
conditions 6361 - 1/4
Al99.5 1) Plates, sheets
and strip
4.1.2 Al-2.5Mg alloy plates - 200 B 209 - - 1745: A 50-451 H 4000 209-1/2
and sheets +200 Alloy 5052 AlMg2.5 5052 A 5052 P AlMg2.5
For general use
under certain 6361 - 1/4
corrosive conditions AlMg2.5
4.1.3 Al-2.7Mg-Mn alloy plates - 200 B 209 - 1470: 5454 1745: A 50-451 H 4000 209-1/2
and sheets +200 Alloy 5454 1) AlMg2.7M 5454 A 5454 P AlMg3Mn
For general use n
under certain 6361 - 1/4
corrosive conditions AlMg3Mn
4.1.4 Al-4.5Mg-Mn alloy plates - 200 B 209 - 1470: 5083 1745: A 50-451 H 4000 209-1/2
and sheets + 65 Alloy 5083 1) AlMg4.5M 5083 A 5083 P AlMg4.5Mn
For low temperature n 0.7
applications 6361 - 1/4
AlMg4.5Mn
4.1.5 Copper plates, sheets - 200 B 152 - 2875: C106 17670: A 51-100 H 3100 1337 - Specify annealed
and strip +150 C12200 1) SF-Cu Cu-b1 C 1220 P Cu-DHP condition for all
For certain corrosive 2870: C106 grades.
conditions 2) 17675: 1634-1/2
SF-Cu Cu-DHP 1) Plates
1)
2) Sheets and
strip
4.1.6 Cu-Zn alloy plates and - 200 B 171 - 2875: 17670: A51-115 H 3100 426-
sheets +175 C46400 CZ112 CuZn38 CuZn38 C 4640 P 1CuZn38Sn 3) Specify
For baffles of coolers 1) Sn1 Sn1 1 Phosphorous
and condensers in 2870: 0.015 max.
brackish and CZ112 17675: 1634-2
seawater service 2) CuZn39S CuZn38Sn1
and for general use n
under certain 1)
corrosive conditions
4.1.7 Cu-Al alloy plates and - 200 B 171 - 2875: 17670: A51-115 H 3100 428 -
sheets +250 C61400 CA106 CuAl8Fe3 CuAl7 C 6140 P CuAl8Fe3
For tube sheets of 1) Fe2 3)
coolers and 17675: 1634-2
condensers in sweet CuAl8Fe CuAl8Fe3
and brackish water 1)
service and for
general use under
certain corrosive
conditions
4.1.8 Cu-Al alloy plates and - 200 B 171 - 2875: 17670: A 51-115 H 3100 428 - Tube sheets
sheets +350 C63000 CA105 CuAl10Ni CuAl9Ni C 6301 P CuAl10Ni5 produced by special
For tube sheets of Al content 1) 5Fe4 5Fe3 Fe4 casting methods
coolers and max. from approved
condensers in 10.0% 17675: 1634-2 manufacturers, are
brackish and CuAl10Ni CuAl10Ni5 acceptable provided
seawater service 1) Fe4 mechanical
and for general use properties and
under certain chemical
corrosive conditions composition are
compatible with this
specification.
1) Plates
4. NON-FERROUS METALS (Cont'd)

4.1 PLATES, SHEETS AND STRIP (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.1.9 Cu-Ni (90/10) alloy - 200 B 171 - 2875: CN102 17670: A51-115 H 3100 429
plates and sheets +350 C70600 1) CuNi10Fe1 CuNi10Fe C 7060 P CuNi10Fe1 1) Plates
For tube sheets of 2870: CN102 Mn 1Mn Mn
coolers and 2) 2) Sheets and
condensers in 17675: 1634-2 strip
brackish and CuNi10Fe CuNi10Fe1
seawater service 1) Mn
and for general use
under certain
corrosive conditions
4.1.10 Cu-Ni (70/30) alloy - 200 B 171 - 2875: CN107 17670: A51-115 H 3100 429
plates and sheets +350 C71500 1) CuNi30Mn CuNi30 C 7150 P CuNi30Mn
For certain corrosive 2870: CN107 1Fe FeMn 1Fe
conditions 2)
17675: 1634-2
CuNi30Fe CuNi30Mn
1) 1 Fe
4.1.11 Nickel plates, sheets and -200 B 162 - 3072: NA11 17750: - H 4551 - Specify annealed
strip (+350) N02200 1) Ni99.2 NNCP condition for all
For certain corrosive 3073: NA11 grades.
conditions 2)
1) Plates and
sheet
4.1.12 Low-carbon nickel - 200 B 162 - 3072: NA12 17750: A54-101 H 4551 -
plates, sheets and strip +350 N02201 1) LC-Ni99 Ni02 NLCP
For certain corrosive 2) Strip
3073: NA12
conditions 2)
3) The material
shall be
capable of
passing the
Practice C
corrosion test
as
4.1.13 Ni-Cu alloy (Monel 400) - 200 B 127 - 3072: NA13 17750: - H 4551 - specified in
plates, sheets and strip +400 N04400 1) NiCu30Fe NCuP ASTM A262.
For certain corrosive 3073: NA13 (Corrosion rate
conditions 2) in this test shall
not exceed
0.3 mm/year).
4.1.14 Ni-Cr-Fe alloy (Inconel +650 B 168 - 3072: NA14 17750: - G 4902 -
600) plates, sheets and N06600 1) NiCr15Fe NCF600
strip 3073: NA14
For high-temp. 2)
conditions and/or
certain corrosive
conditions
4.1.15 Ni-Fe-Cr alloy (Incoloy +815 B 409 - 3072: NA15 SEW 470: G 4902 -
800) plates, sheets and N08800 1) X 10 NiCr NCF 800
strip 3073: NA15 AlTi32 20
For high-temp. 2)
conditions and/or
certain corrosive
conditions
4.1.16 Ni-Fe-Cr alloy (Incoloy +1000 B 409 - 3072: - - G 4902 -
800H) plates, sheets and N08810 NA15(H) NCF
strip 1) 800H
For high-temp.
conditions and/or
certain corrosive
conditions
4. NON-FERROUS METALS (Cont'd)

4.1 PLATES, SHEETS AND STRIP (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.1.17 Ni-Fe-Cr alloy (Incoloy (+1000) B 409 - - - - - - 1) Plates and
800HT) plates, sheets and N08811 sheet
strip 2) Strip
For high-temp.
conditions and/or
certain corrosive
conditions
4.1.18 Ni-Fe-Cr-Mo-Cu alloy +425 B 424 - 3072: NA16 17750: - G 4902 - 3) The material
(Incoloy 825) plates, sheets N08825 1) 3) NiCr21Mo NCF 825 shall be
and strip 3) 3073: NA16 3) 3) capable of
For certain corrosive 2) 3) passing the
conditions Practice C
intergranular
corrosion test
as specified in
ASTM A262
(Corrosion rate
in this test shall
not exceed
0.3 mm/year).
4.1.19 Ni-Cr-Mo-Nb alloy (Inconel +425 B 443 - 3072: NA21 17750: - - -
625) plates, sheets and N06625 1) NiCr22Mo
strip 3073: NA21 9Nb
For certain corrosive 2)
conditions
4.1.20 Ni-Mo alloy (Hastelloy B2) +425 B 333 - - 17750: - - -
plates, sheets and strip N10665 NiMo28
For certain corrosive
conditions
4.1.21 Ni-Mo-Cr alloy (Hastelloy +425 B 575 - - 17750: - - -
C4) plates, sheets and N06455 NiMo16Cr
strip 16Ti
For certain corrosive
conditions
4.1.22 Ni-Mo-Cr alloy (Hastelloy +425 B 575 - - 17750: A54-401 - -
C276) plates, sheets and (+650) N10276 NiMo16Cr Ni-Mo16
strip 15W Cr15
For certain corrosive
conditions
4.1.23 Ni-Cr-Mo alloy (Hastelloy (+425) B 575 - - - - - -
C22) plates, sheets and N06022
strip
For certain corrosive
conditions
4.1.24 Titanium plates, sheets (+300) B 265 - - 17860: - H 4600 - 1) For linings,
and strip Grade 2 Ti2 TP 35H or tensile
For certain corrosive 1) 2) 1) 2) C properties
conditions 1) 2) indicated in the
material
specifications to
be used for
information
only.
Specify soft-
annealed
material with
hardness 140
HV10 max.
2) The softer
Grade 1 may
also be used for
lining.
4. NON-FERROUS METALS (Cont'd)

4.1 PLATES, SHEETS AND STRIP (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.1.25 Tantalum plates, 2) B 708 - - - - H 4701 - 1) For linings,
sheets and strip R05200 TaP tensile
For certain 1) 1) properties
corrosive indicated in the
conditions material
specifications to
be used for
information
only.
Specify soft-
annealed
material with
hardness 120
HV10 max.
2) Temperature
limits depend
on nature of
services.
4. NON-FERROUS METALS (Cont'd)

4.2 TUBES AND TUBING


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.2.1 Seamless aluminium - 200 B 234 - 1471: 1050A 1795: A 50-411 H 4080 209-1/2 Specify annealed
tubes +200 Alloy 1060 Al99.5 1050A A 1050 Al 99.5 condition for all
For unfired heat TD grades.
transfer TR2778
equipment under Al99.5
certain corrosive
conditions
4.2.2 Seamless Al-2.5 Mg - 200 B 234 - - - A 50-411 H 4080 209-1/2
alloy tubes +200 Alloy 5052 5052 A 5052 AlMg 2.5
For unfired heat TD
transfer TR2778
equipment under AlMg2.5
certain corrosive
conditions

4.2.3 Seamless Al-2.7 Mg- - 200 B 234 - - 1795: - - 209-1/2


Mn alloy tubes +200 Alloy 5454 AlMg3 AlMg3Mn
For unfired heat
transfer
equipment under
certain corrosive
conditions
4.2.4 Seamless copper - 200 B 68 - 2871: Part 2 - 17671: A 51-124 H 3300 1635- Specify annealed
tubing in small sizes +150 C12200 C106 SF-Cu Cu-DHP C 1220 Cu DHP condition for all
For instrument 06 O grades.
lines
4.2.5 Seamless Cu-Zn-Al (- 200) B 111 - 2871: Part 3 - 1785: A 51-102 H 3300 1635-2
alloy (Aluminium +175 C68700 CZ110 CuZn20Al2 CuZn22 C 6870 CuZn20Al2
Brass) tubes F34 Al2
For coolers and
condensers in
brackish and
seawater service

4.2.6 Seamless copper - 200 B 111 - 2871: Part 3 - 1785: A 51-102 H 3300 1635-2
nickel (90/10 Cu-Ni) +350 C70600 CN102 CuNi10Fe CuNi10 C 7060 CuNi10Fe
alloy tubes 1Mn F29 Fe 1 Mn 1Mn
For unfired heat
transfer
equipment under
certain corrosive
conditions

4.2.7 Seamless copper - 200 B 111 - 2871: Part 3 - 1785: A 51-102 H 3300 1635-2
nickel (70/30 Cu-Ni) +350 C71500 CN107 CuNi30Mn CuNi30 C 7150 CuNi30Mn
alloy tubes 1Fe F37 Mn 1 Fe 1Fe
For unfired heat
transfer
equipment under
certain corrosive
conditions
4.2.8 Seamless copper - 200 B 111 - 2871: Part 3 - 1785: A 51-102 H 3300 1635-2
nickel (66/30/2/2 Cu- +350 C71640 CN108 CuNi30Fe CuNi30 C 7150 CuNi30Mn
Ni-Fe-Mn) alloy tubes. 2Mn 2F42 Fe2 Mn2 1Fe
For unfired heat
transfer
equipment under
certain corrosive
conditions
4. NON-FERROUS METALS (Cont'd)

4.2 TUBES AND TUBING (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.2.9 Seamless nickel -200 B 163 - 3074: NA11 17751: - - - Specify solution
tubes +350 N02200 Ni99.2 annealed condition
For unfired heat F37 for all grades.
transfer
equipment under For tubes intended
certain corrosive for use with
conditions compression
fittings, hardness
shall not exceed 90
HRB.
4.2.10 Seamless low-carbon - 200 B 163 - 3074: NA12 17751: - - -
nickel tubes +350 N02201 LC-Ni99
For unfired heat F34
transfer
equipment under
certain corrosive
conditions

4.2.11 Seamless Ni-Cu alloy - 200 B 163 - 3074: NA13 17751: - H 4552 -
(Monel 400) tubes +400 N04400 NiCu30Fe NCuT
For unfired heat F45
transfer
equipment under
certain corrosive
conditions
4.2.12 Seamless Ni-Cr-Fe +650 B 163 - 3074: NA14 17751: - G 4904 -
alloy (Inconel 600) N06600 NiCr15Fe NCF 600
tubes F50 TB
For unfired heat
transfer
equipment under
certain corrosive
conditions

4.2.13 Seamless Ni-Fe-Cr +815 B 163 - 3074: NA15 SEW 470: - G 4904 -
alloy (Incoloy 800) N08800 X 10 NiCr NCF 800
tubes AlTi 32 20 TB
For unfired heat
transfer
equipment under
certain corrosive
conditions

4.2.14 Seamless Ni-Fe-Cr +1000 B 407 - 3074: NA15 - - G 4904 -


alloy (Incoloy 800H) N08810 (H) NCF 800
tubes HTB
For furnaces and
unfired heat
transfer
equipment under
certain corrosive
conditions

4.2.15 Seamless Ni-Fe-Cr (+1000) B 407 - - - - - -


alloy (Incoloy 800 HT) N08811
tubes
For furnaces and
unfired heat
transfer
equipment under
certain corrosive
conditions
4. NON-FERROUS METALS (Cont'd)

4.2 TUBES AND TUBING (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.2.16 Seamless Ni-Fe-Cr-Mo- (-200) B 163 - 3074: NA16 17751: - G 4904 Specify solution
Cu alloy (Incoloy 825) +425 N08825 NiCr21Mo NCF 825 annealed condition
tubes F55 TB for all grades.
For unfired heat
transfer equipment For tubes intended
under certain for use with
corrosive conditions compression
fittings, hardness
shall not exceed 90
HRB.
4.2.17 Seamless Ni-Cr-Mo-Nb +425 B 444 - 3074: NA21 17751: - - -
alloy (Inconel 625) tubes N06625 NiCr22Mo9
For unfired heat NbF69
transfer equipment
under certain
corrosive conditions
4.2.18 Seamless Ni-Mo alloy +425 B 622 - - 17751:
(Hastelloy B2) tubes N10665 NiMo28
For unfired heat
transfer equipment
under certain
corrosive conditions
4.2.19 Welded Ni-Mo alloy +425 B 626 - - - - - -
(Hastelloy B2) tubes N10665
For unfired heat Class 1A
transfer equipment
under certain
corrosive conditions
4.2.20 Seamless Ni-Mo-Cr alloy +425 B 622 - - 17751: - - -
(Hastelloy C4) tubes N06455 NiMo16Cr
For unfired heat 16Ti
transfer equipment
under certain
corrosive conditions

4.2.21 Welded Ni-Mo-Cr alloy +425 B 626 - - - - - -


(Hastelloy C4) tubes N06455
For unfired heat Class 1A
transfer equipment
under certain
corrosive conditions

4.2.22 Seamless Ni-Mo-Cr alloy +425 B 622 - - 17751: - - -


(Hastelloy C276) tubes (+650) N10276 NiMo16Cr
For unfired heat 15W
transfer equipment
under certain
corrosive conditions

4.2.23 Welded Ni-Mo-Cr alloy +425 B 626 - - - - - -


(Hastelloy C276) tubes (+650) N10276
For unfired heat Class 1A
transfer equipment
under certain
corrosive conditions
4. NON-FERROUS METALS (Cont'd)

4.2 TUBES AND TUBING (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.2.24 Seamless Ni-Cr-Mo (+425) B 622 - - - - - -
alloy (Hastelloy C22) N06022
tubes
For unfired heat
transfer
equipment under
certain corrosive
conditions
4.2.25 Welded Ni-Cr-Mo (+425) B 626 - - - - - -
alloy (Hastelloy C22) N06022
tubes Class 1A
For unfired heat
transfer
equipment under
certain corrosive
conditions
4.2.26 Seamless titanium (+300) B 338 - - 17861: - H 4631: -
tubes Grade 2 Ti2 TTH 35 D
For unfired heat
transfer
equipment under
certain corrosive
conditions

4.2.27 Welded titanium (+300) B 338 - - 17866: - H 4631: -


tubes Grade 2 Ti2 TTH 35
For unfired heat WD
transfer
equipment under
certain corrosive
conditions
4. NON-FERROUS METALS (Cont'd)

4.3 PIPE
DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.3.1 Seamless aluminium - 200 B 241 - 1474: 1050A 9107: A 50-411 H 4080 209-1/2 Specify annealed
pipe +200 Alloy 1060 Al99.5 1050A A 1050 Al 99.5 condition for all
For certain TD grades.
corrosive
conditions
4.3.2 Seamless Al-Mg-Si - 200 B 241 - 1474: 6061 - A 50-411 H 4080 209-1/2
alloy pipe +200 Alloy 6061 6061 A 6061 AlMg1SiCu
For certain TD
corrosive
conditions
4.3.3 Seamless Al-Mg-Si - 200 B 241 - 1474: 6063 9107: - H 4080 209-1/2
alloy pipe +200 Alloy 6063 AlMgSi 0.5 A 6063 AlMg0.7Si
For pipelines TD
under certain
corrosive
conditions
4.3.4 Seamless Al-2.5Mg - 200 B 241 - - - A 50-411 H 4080 209-1/2
alloy pipe +200 Alloy 5052 5052 A 5052 AlMg 2.5
For general use TD
under certain
corrosive
conditions
4.3.5 Seamless Al-2.7Mg- - 200 B 241 - - 9107: - - 209-1/2
Mn alloy pipe +200 Alloy 5454 AlMg3 AlMg3Mn
For general use
under certain
corrosive
conditions

4.3.6 Seamless Al-4.5Mg- - 200 B 241 - 1474: 5083 9107: A 50-411 H 4080 209-1/2
Mn alloy pipe + 65 Alloy 5083 AlMg4.5Mn 5083 A 5083 AlMg4.5Mn
For low- TD 0.7
temperature
service only.
4.3.7 Seamless copper - 200 B 42 - 2871: Part 2 - 17671: A 51-124 H 3300 1635 - Specify annealed
pipe +150 C12200 C106 SF-Cu Cu/b C1220 Cu-DHP condition for all
For certain grade.
corrosive
conditions
4.3.8 Seamless Cu-Zn-Al (-200) B111 2871: Part 2 - 17671: - H 3300 1635 -
alloy (Aluminium +175 C68700 CZ110 CuZn20Al2 C 6870 CuZn20Al2
Brass) pipe
For brackish and
seawater service

4.3.9 Seamless Cu-Ni alloy (-200) B 466 - 2871: Part 2 - 17671: - H 3300 1635 -
(90/10 Cu-Ni) pipe +350 C70600 CN102 CuNi10Fe C 7060 CuNi10Fe
For seawater 1Mn 1Mn
service
4.3.10 Seamless Cu-Ni alloy -200 B 466 - 2871: Part 2 - 17671: - H 3300 1635 -
(70/30 Cu-Ni) pipe +350 C71500 CN107 CuNi30Mn C 7150 CuNi30Mn
For certain 1Fe 1Fe
corrosive
conditions
4. NON-FERROUS METALS (Cont'd)

4.3 PIPE (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.3.11 Seamless nickel pipe -200 B 161 - 3074: NA11 17751: - H 4552 - Specify cold-
For certain +350 N02200 Ni99.2 NNCT-0 worked, annealed
corrosive F37 and pickled
conditions condition for all
grades.
4.3.12 Seamless low-carbon - 200 B 161 - 3074: NA12 17751: - H 4552 - 1) See DEP
nickel pipe +350 N02201 LC-Ni99 NLCT-0 31.24.40.31-
For certain F34 Gen.
corrosive
conditions
4.3.13 Seamless Ni-Cu alloy -200 B 165 - 3074: NA13 17751: - H 4552 - 2) The material
(Monel 400) pipe +400 N04400 NiCu30Fe NCu T-0 shall be
For certain F45 capable of
corrosive passing the
conditions Practice C
intergranular
corrosion test
as specified in
ASTM A262.
(Corrosion rate
in this test shall
not exceed
0.3 mm/year).
4.3.14 Seamless Ni-Cr-Fe +650 B 167 - 3074: NA14 17751: - G 4903 -
alloy (Inconel 600) N06600 NiCr15Fe NCF 600
pipe F50 TP
For high
temperature
conditions and/or
certain corrosive
conditions
4.3.15 Seamless Ni-Fe-Cr (-200) B 407 - 3074: NA15 SEW 470: - G 4903 -
alloy (Incoloy 800) +815 N08800 X10NiCr NCF 800
pipe AlTi32 20 TP
For high
temperature
conditions and/or
certain corrosive
conditions
4.3.16 Seamless Ni-Fe-Cr +1000 B 407 - 3074: - - G 4903 -
alloy (Incoloy 800H) 1) N08810 NA15(H) NCF 800
pipe HTP
For high
temperature
conditions and/or
certain corrosive
conditions

4.3.17 Seamless Ni-Fe-Cr (+1000) B 407 - - - - -


alloy (Incoloy 800HT) 1) N08811
pipe
For high
temperature
conditions and/or
certain corrosive
conditions

4.3.18 Seamless Ni-Fe-Cr- (-200) B 423 - 3074: NA16 17751: - G 4903 -


Mo-Cu alloy (Incoloy +425 N08825 2) NiCr21Mo NCF 825
825) pipe 2) F55 TP
For certain 2) 2)
corrosive
conditions
4. NON-FERROUS METALS (Cont'd)

4.3 PIPE (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.3.19 Welded Ni-Fe-Cr-Mo-Cu (-200) B705 - - - - - - Specify cold-worked
alloy (Incoloy 825) pipe +425 N08825 and bright annealed
For certain corrosive Class 2 condition.
conditions 1)
1) The material
shall be
capable of
passing the
Practice C
intergranular
corrosion test
as specified in
ASTM A262.
(Corrosion rate
in this test shall
not exceed
0.3 mm/year).
4.3.20 Seamless Ni-Cr-Mo-Nb +425 B 444 - 3074: NA21 17751: - - - Specify cold-worked
alloy (Inconel 625) pipe N06625 NiCr22Mo and bright annealed
For certain corrosive 9NbF69 condition for all
conditions grades.

4.3.21 Welded Ni-Cr-Mo-Nb +425 B705 - - - - - - Specify cold-worked


alloy (Inconel 625) pipe N06625 and bright annealed
For certain corrosive Class 2 condition.
conditions
4.3.22 Seamless Ni-Mo alloy +425 B 622 - - 17751: - - -
(Hastelloy B2) pipe N10665 NiMo28
For certain corrosive
conditions

4.3.23 Welded Ni-Mo alloy +425 B 619 - - - - - -


(Hastelloy B2) pipe N10665
For certain corrosive Class II
conditions
4.3.24 Seamless Ni-Mo-Cr alloy +425 B 622 - - 17751: - - -
(Hastelloy C4) pipe N06455 NiMo16Cr
For certain corrosive 16Ti
conditions

4.3.25 Welded Ni-Mo-Cr alloy +425 B 619 - - - - - -


(Hastelloy C4) pipe N06455
For certain corrosive Class II
conditions
4.3.26 Seamless Ni-Mo-Cr alloy +425 B 622 - - 17751: - - -
(Hastelloy C276) pipe (+650) N10276 NiMo16Cr
For certain corrosive 15W
conditions

4.3.27 Welded Ni-Mo-Cr alloy +425 B 619 - - - - - -


(Hastelloy C276) pipe (+650) N10276
For certain corrosive Class II
conditions
4. NON-FERROUS METALS (Cont'd)

4.3 PIPE (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.3.28 Seamless Ni-Cr-Mo (+425) B 622 - - - - - -
alloy (Hastelloy C22) N06022
pipe
For certain
corrosive
conditions

4.3.29 Welded Ni-Cr-Mo (+425) B 619 - - - - -


alloy (Hastelloy C22) N06022
pipe Class II
For certain
corrosive
conditions

4.3.30 Seamless titanium (+300) B 337 - - 17861: - H 4630: - 1) Specify bright


pipe Grade 2 Ti2 TTP 35D annealed
For certain 1) 1) condition for
corrosive seamless and
conditions welded.

4.3.31 Welded titanium pipe (+300) B 337 - - 17866: - H4630: -


For certain Grade 2 Ti2 TTP
corrosive 1) 35WD
conditions 1)
4. NON-FERROUS METALS (Cont'd)

4.4 FORGINGS, FLANGES AND FITTINGS


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.4.1 Al-2.5Mg alloy forgings -200 Alloy 5052 - - - - 209-1/2 Specify annealed
For general use +200 1) AlMg2.5 condition for all
under certain grades.
corrosive conditions
4.4.2 Al-2.7Mg-Mn alloy -200 Alloy 5454 - - - 209-1/2 1) Order to
forgings +200 1) AlMg3Mn ASTM B 247,
For general use with reference
under certain to
corrosive conditions ASME VIII,
Div. 1, para
UG 15.
4.4.3 Al-4.5Mg-Mn alloy -200 B 247 - 1472: NF8 1749: A50-901 H 4140 209-1/2 2) Order to
forgings + 65 Alloy 5083 AlMg4.5Mn 5083 A 5083 AlMg4.5Mn ASTM B 361,
For low-temperature FD or FH 0.7 with reference
service only. to
ASME VIII,
Div. 1, para
UG 15.
4.4.4 Al-Mg-Si alloy forgings -200 B 247 - - - A50-901 H 4140 209-1/2
For certain corrosive +200 Alloy 6061 6061 A 6061 AlMg1SiCu
conditions and/or FD or FH
low-temperature
service.

4.4.5 Al-Mg-Si alloy welding -200 B 361 - - - - - -


fittings +200 WP 6061
For certain corrosive
conditions and/or
low-temperature
service.

4.4.6 Al-2.5Mg alloy welding -200 Alloy - - - - -


fittings +200 WP 5052
For use in marine or
atmosphere and for WP 5052W
general use under 2)
certain corrosive
conditions
4.4.7 Al-2.7Mg-Mn alloy -200 Alloy - - - - -
welding fittings +200 WP 5454
For use in marine or
atmosphere and for WP 5454W
general use under 2)
certain corrosive
conditions

4.4.8 Nickel welding fittings. (+325) B 366 - - - - - -


For certain corrosive WPNS or
conditions WPNW

4.4.9 Low-carbon nickel (+600) B 366 - - - - - -


welding fittings WPNLS or
For certain corrosive WPNLW
conditions
4.4.10 Ni-Cu alloy (Monel 400) -200 B 564 - - - - - -
forgings. +400 N04400
For certain corrosive
conditions
4. NON-FERROUS METALS (Cont'd)

4.4 FORGINGS, FLANGES AND FITTINGS (CONT'D)


DESIGNATION AND Metal ASTM BS DIN AFNOR JIS ISO REMARKS
APPLICATION Temp., °C
(See 1.7)
4.4.11 Ni-Cu alloy (Monel 400) -200 B 366 - - 17754: - - Specify solution
welding fittings +400 WPNCS or NiCu30Fe annealed condition
For certain corrosive WPNCW for all grades.
conditions
4.4.12 Ni-Cu alloy (Monel) 400) +650 B 564 - - - - - - 1) See DEP
forgings N06600 31.24.40.31-
For high temperature Gen.
conditions and/or
certain corrosive 2) The material
conditions shall be capable
of passing the
Practice C
intergranular
corrosion test as
specified in
ASTM A262.
(Corrosion rate
in this test shall
not exceed
0.3 mm/year).
4.4.13 Ni-Cr-Fe alloy (Inconel +650 B 366 - - - - - -
600) fittings WPNC1S
For high temperature or
conditions and/or WPNC1W
certain corrosive
conditions
4.4.14 Ni-Fe-Cr alloy (Incoloy +815 B 564 - - - - - -
800) forgings Alloy
For extreme N08800
temperature service
4.4.15 Ni-Fe-Cr alloy (Incoloy +1000 B 564 - - - - - -
800H) forgings 1) N08810
For extreme
temperature service
4.4.16 Ni-Fe-Cr-Mo-Cu alloy (-200) B 564 - - - - - -
(Incoloy 825) forgings +450 N08825
For extreme 2)
temperature service
4.4.17 Ni-Fe-Cr-Mo-Cu alloy (-200) B 366 - - - - - -
(Incoloy 825) weldng +450 WPNI
fittings CMCS or
For extreme WPNI
temperature service CMCW
2)
4.4.18 Ni-Mo alloy (Hastelloy B2) +425 B 366 - - 17754: - - -
welding fittings WPHB2S NiMo30
For certain corrosive or
conditions WPHB2W
4.4.19 Ni-Mo-Cr alloy (Hastelloy +425 B 366 - - - - - -
C4) welding fittings WPHC4
For certain corrosive
conditions
4.4.20 Ni-Mo-Cr alloy (Hastelloy (+800) B 366 - - - - - -
C276) welding fittings WPHC276
For certain corrosive
conditions
4.4.21 Ni-Cr-Mo alloy (Hastelloy (+425) B 564 - - - - - -
C22) forgings N06022
For certain corrosive
conditions
4. NON-FERROUS METALS (Cont'd)

4.4 FORGINGS, FLANGES AND FITTINGS (CONT'D)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.4.22 Ni-Cr-Mo alloy +425 B 366 - - - - - - Specify solution
(Hastelloy C22) WPHC22S annealed condition
welding fittings or for all grades.
For certain WPHC22W
corrosive
conditions

4.4.23 Titanium forgings (+300) B 381 - - 17864: - - - Specify annealed


For certain Grade F2 Ti2 conditon for all
corrosive grades.
conditions
4.4.24 Titanium welding (+300) B 363 - - - - - -
fittings WPT2 or
For certain WPT2W
corrosive
conditions
4. NON-FERROUS METALS (Cont'd)
4.5 CASTINGS
Amended per
Circular 35/98

DESIGNATION AND Metal


APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.5.1 Al-5Si alloy castings -200 B 26 - - - - - - 1) Specify B108
For certain +200 Alloy Alloy B443.0 for
corrosive B443.0 permanent
conditions 1) mould castings.
4.5.2 Al-12Si alloy castings -200 - 1490: LM6 1725: A57-702 H 5202 3522
For certain +200 G-AlSi12 A-S13 AC3A Al-Si12
corrosive
conditions
4.5.3 Composition bronze -200 B 62 - 1400: LG2C 1705: A53-707 H 5111 - 1) Lead content
(Bronze 85/5/5/5) +175 C83600 G-CuSn5 CuSn5 BC6 0.3% max.
castings ZnPb Pb5Zn5
For flanges,
fittings and valves
4.5.4 Tin bronze (Bronze -200 B 584- 1400: G1 1705: - H 5111 -
88/10/2) castings +175 C90500 1) G-CuSn10 BC3
For equipment Zn
parts to be used 1)
in brackish and
seawater service
and for certain
corrosive
conditions
4.5.5 Ni-Al bronze castings -200 B 148 - 1400: AB2 1714: A53-709 H 5114 -
For equipment +350 C95800 G-CuAl10 CuAl10 Al BC3
parts to be used 2) Ni Fe5Ni5
in brackish and
seawater service
and for certain
corrosive
conditions

4.5.6 Lead in pig form +100 B 29 - 334: Type A 1719: A55-105 - -


For homogeneous Chemical - Pb99.9Cu Pb doux
linings of Copper Raffiné
equipment under Lead UNS 99.90
certain corrosive L551121
conditions
4.5.7 Ni-Cu alloy -200 A 494 - 3071: NA1 17730: - -
(Monel 400) castings +400 M35-1 G-NiCu30
For certain Nb
corrosive
conditions

4.5.8 Ni-Mo alloy +425 A494 - - - - - -


(Hastelloy B2) N-7M
castings Class 1
For certain
corrosive
conditions

4.5.9 Ni-Mo-Cr alloy +425 A494 - - - - - -


(Hastelloy C4) CW-2M
castings
For certain
corrosive
conditions
4. NON-FERROUS METALS (Cont'd)

4.5 CASTINGS (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.5.10 Ni-Mo-Cr alloy +425 A494 - - - - - -
(Hastelloy C276) (+650) CW-12MW
castings Class 1
For certain
corrosive
conditions

4.5.11 50Cr-50Ni-Nb alloy +1000 A560 - - - - - -


castings 50Cr-50Ni-
For furnace tube Cb
supports exposed
to vanadium
attack

4.5.12 Titanium castings (+250) B367 - - 17865: - - -


For certain Grade C2 G-Ti2
corrosive
conditions
4. NON-FERROUS METALS (Cont'd)

4.6 BARS, SECTIONS AND WIRE


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.6.1 Extruded aluminium -200 B 221 - 1474: 1050A 1747: A50-411 H 4040 209-1/2 For bars, rods and
bars, rods, sections +200 Alloy 1060 1) Al99.5 1050A A 1050 Al99.5 sections, specify
(incl. hollow sections), 2) BE annealed condition
tube and wire 6362-1/4 for all grades.
For certain Al99.5 For wire, condition
corrosive to be agreed upon
conditions for each case
individually.
4.6.2 Extruded Al-2.5 Mg -200 B 221 - - - A 50-702 H 4040 209-1/2 1) Bars, extruded
alloy bars, rods, +200 Alloy 5052 5052 A 5052 AlMg2.5 sections (incl.
sections (incl. hollow BE hollow section)
sections), tube and and tube.
wire H 4100
For general use A 5052S 2) Bars and rods.
under certain 3)
corrosive
conditions

4.6.3 Extruded Al-2.7 Mg- -200 B 221 - - 1747: A 50-411 H 4100 209-1/2 3) Extruded
Mn alloy bars, rods, +200 Alloy 5454 AlMg3 5454 A 5454 S AlMg3Mn sections.
sections (incl. hollow 2) 3)
sections), tube and 6362-1/4
wire AlMg3Mn
For general use
under certain
corrosive
conditions

4.6.4 Extruded Al-Mg-Si -200 B 221 - 1474: 6063 1747: - H 4040 209-1/2
alloy bars, rods, +200 Alloy 6063 1) AlMgSi0.5 A 6063 AlMg0.7Si
sections (incl. hollow 2) BE
sections), tube and
wire H 4100 6362-1/4
For general A 6063S AlMg0.75i
purposes 3)
4.6.5 Copper bars, rods -200 B 133 - 2874: C101 40500: - H 3250 1637 - For bars, rods and
and sections +150 C11000 SE-Cu C 1100 Cu- sections, specify
For electrical BEC or ETP annealed condition
purposes BED for all grades.
For wire, condition
to be agreed upon
foreach case
individually.
4.6.6 Copper bars, rods -200 B 133 - 2874: C106 17672: - H 3250 1637 -
and sections +150 C12200 SF-Cu C1220 Cu-
For general BE or BD DHP
purposes
4.6.7 Free cutting Cu-Zn -200 B 16 - 2874: 17672: A 51-105 H 3250 1637 -
alloy bars, rods and +175 C36000 CZ124 CuZn36 CuZn36 C 3602 CuZn36
sections Pb3 Pb3 BE or BD Pb3
For general
purposes
4.6.8 Cu-Zn-Pb alloy bars, -200 B140 - - - - - -
rods and sections +150 C32000 or
For general purposes C31400
4. NON-FERROUS METALS (Cont'd)

4.6 BARS, SECTIONS AND WIRE (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.6.9 Cu-Al alloy bars, rods -200 B 150 - 2874: 17672: A 51-116 - 1637 -
and sections +350 C63200 CA104 CuAl10Ni CuAl10Ni CuAl10Ni
For general Al content 5Fe4 5Fe4 5 Fe4
purposes under max. 10.0%
certain corrosive
conditions

4.6.10 Cu-Ni (90/10) alloy bars, -200 B 122 - 2874: CN102 17672: - - -
rods and sections +350 C706 CuNi10Fe
For certain corrosive 1Mn
conditions
4.6.11 Cu-Ni (70/30) alloy bars, -200 B 122 - 2874: CN107 17672: - - 1637 -
rods and sections +350 C71500 CuNi30Mn CuNi30Mn
For certain corrosive 1Fe 1Fe
conditions

4.6.12 Phosphor bronze wire -200 B 159 - 2873: PB102 17682: A 51-111 H3270 1638 -
For springs +175 C51000 Condition H CuSn6F95 CuSn6P C5102 CuSn5
Condition W-H
H08
(Spring
Temper)
4.6.13 Nickel bars and rods (+325) B 160 - 3076: NA11 17752: - H 4553 - For bars and rods,
For certain corrosive N02200 Ni99.2 NNCB specify solution
conditions annealed condition
for all grades,
4.6.14 Low-carbon nickel bars -200 B 160 - 3076: NA12 17752: - H 4553 - except Monel K500
and rods +350 N02201 LC-Ni99 NLCB which should be
For certain corrosive supplied in the
conditions solution treated and
precipitation
hardened condition.
4.6.15 Ni-Cu alloy -200 B 164 - 3076: NA13 17752: - H 4553 - For wire, condition
(Monel 400) bars, rods +400 N04400 1) NiCu30Fe NCuB to be agreed upon
and wire 3075: NA13 for each case
For certain corrosive 2) individually.
conditions 1) Bar
4.6.16 Ni-Cu-Al alloy -200 - 3076: NA18 17752: - H 4553 - 2) Wire
(Monel K500) bars, rods +400 1) NiCu30Al NCu ATB
and wire 3075: NA18
For certain corrosive 2)
conditions requiring
high tensile strength
4.6.17 Ni-Cr-Fe alloy +650 B 166 - 3076: NA14 17752: - G 4901 -
(Inconel 600) bars, rods N06600 1) NiCr15Fe NCF 600
and wire 3075: NA14
For high- 2)
temperature
conditions and/or
certain corrosive
conditions
4.6.18 Ni-Cr-Mo-Nb alloy +425 B 446 - 3076: NA21 17752: - - -
(Inconel 625) bars and N06625 1) NiCr22Mo
rods 9Nb
For certain corrosive
conditions
4. NON-FERROUS METALS (Cont'd)

4.6 BARS, SECTIONS AND WIRE (Cont'd)


DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.6.19 Ni-Fe-Cr alloy +815 B 408 - 3076: NA15 SEW 470: - G 4901 - 1) Bar
(Incoloy 800) bars, N08800 1) X10 NiCr NCF 800
rods and wire 3075: NA15 AlTi32 20 2) Wire
For high- 2)
temperature
conditions and/or
certain corrosive
conditions
4.6.20 Ni-Fe-Cr alloy +1000 B 408 - 3076: - - G 4901 -
(Incoloy 800H) bars, N08810 NA15(H) NCF
rods and wire 1) 800H
For high-
temperature
conditions and/or
certain corrosive
conditions
4.6.21 Ni-Fe-Cr alloy (+1000) B 408 - - - - - -
(Incoloy 800HT) bars, N08811
rods and wire
For high-
temperature
conditions and/or
certain corrosive
conditions
4.6.22 Ni-Fe-Cr-Mo-Cu alloy (+425) B 425 - 3076: NA16 17752: - G 4901 -
(Incoloy 825) bars, N08825 1) NiCr21Mo NCF 825
rods and wire
For certain
corrosive
conditions
4.6.23 Ni-Mo alloy (Hastelloy +425 B 335 - - 17752: - H 4553 -
B2) rods N10665 NiMo28 NM 2B
For certain
corrosive
conditions

4.6.24 Ni-Mo-Cr alloy +425 B 574 - - 17752: - - -


(Hastelloy C4) rods N06455 NiMo16Cr
For certain 16Ti
corrosive
conditions

4.6.25 Ni-Mo-Cr alloy (+800) B 574 - - 17752: A54-401 H 4553 -


(Hastelloy C276) rods N10276 NiMo16Cr Ni-Mo16 NM Cr B
For certain 15W Cr15
corrosive
conditions
4.6.26 Ni-Cr-Mo alloy (+425) B 574 - - - - - -
(Hastelloy C22) rods N06022
For certain
corrosive
conditions
4.6.27 Titanium bars (+300) B 348 - - 17862: - H 4650 - Specify annealed
For certain Grade 2 Ti2 TB35 condition.
corrosive H or C
conditions
4. NON-FERROUS METALS (Cont'd)

4.7 BOLTING
DESIGNATION AND Metal
APPLICATION Temp., °C ASTM BS DIN AFNOR JIS ISO REMARKS
(See 1.7)
4.7.1 Aluminium alloy bolts -200 F467/468 - - - - - - Bolting material
and nuts +200 A96061 may also be
selected from
Section 4.6.
4.7.2 Cu-Al alloy bolts and -200 F467/468 - - - - - -
nuts +365 C63000

4.7.3 Cu-Ni (70/30) alloy -200 F467/468 - - - - - -


bolts and nuts +350 C71500

4.7.4 Ni-Cu alloy -200 F467/468 - - - - - -


(Monel 400) bolts +400 N04400
and nuts

4.7.5 Ni-Cu-Al alloy (Monel -200 F467/468 -


K500) bolts and nuts +400 N05500

4.7.6 Ni-Mo alloy +425 F467/468 - - - - - -


(Hastelloy B) bolts N10001
and nuts

4.7.7 Ni-Mo-Cr alloy (+800) F467/468 - - - - -


(Hastelloy C276) bolts N10276
and nuts

4.7.8 Titanium bolts and (+300) F467/468 - - - - - - Bolts primarily


nuts Alloy Ti 2 intended for use
inside equipment.
5. REFERENCES

In this DEP reference is made to the following publications:

NOTES: 1. Unless specifically designated by date, the latest edition of each publication shall be used,
together with any amendments/supplements/revisions thereto.
2. The numerous materials standards found in sections 2 to 4 have not separately been listed here,
but the organisation addresses are given.

SHELL STANDARDS

Index to DEP publications and standard DEP 00.00.05.05-Gen.


specifications

Metallic Materials - Requirements for prevention of DEP 30.10.02.31-Gen.


brittle fracture of equipment in low-temperature
service (45 °C or below) and equipment containing
liquefied gas or lethal substances

Selected materials for furnace parts for high- DEP 31 24.40.31-Gen.


temperature conversion processes

Standard vertical tanks - Selection, design and DEP 34.51.01.31-Gen.


fabrication

AMERICAN STANDARDS

Steels for Hydrogen Service at Elevated API 941


Temperatures and Pressures in Petroleum
Refineries and Petrochemical Plants
Issued by:
American Petroleum Institute
Publications and Distribution Section
2101 L Street Northwest
Washington, DC 20037
USA.

ASTM standards
NOTE: Where metric versions of ASTM standards are available (e.g. ASTM A278M) they should be selected.
In most cases, ASTM standards and their metric version are issued as a single standard (e.g. ASTM
A182/A182M).

Issued by:
American Society for Testing and Materials
1916 Race St., Philadelphia
Pa. 19103, USA.

BRITISH STANDARDS

BSI standards
Issued by:
British Standards Institution
389 Chiswick High Road
London W4 4AL
England
United Kingdom.
EUROPEAN STANDARDS

CEN standards

Issued by:
Committé Européen de Normalisation
Secrétariat Central
Rue de Stassart 36
B-1050 Brussels
Belgium
Copies can also be obtained from national standards
organizations

FRENCH STANDARDS

AFNOR standards
Issued by:
AFNOR
19 Rue de 4 Septembre
Paris (2e), France.

GERMAN STANDARDS

DIN Normen
Issued by:
Beuth Verlag GmbH
Burggrafenstrasse 4-10
1000 Berlin 30, Germany.

SEW Blätter
Issued by:
Verein Deutscher Eisenhüttenleute
Verlag Stahleisen m.b.H
P.O. Box 8229
4-Düsseldorf, Germany.

INTERNATIONAL STANDARDS
ISO standards
Issued by:
International Organization for Standardization
1, Rue de Varembé
CH-1211 Geneva 20
Switzerland.

NOTE: Copies can also be obtained from national standards organizations

JAPANESE STANDARDS

JIS standards
Issued by:
Japanese Standards Association
1-24 Akasaka 4 Chome
Minato - ku
Tokyo, Japan.
APPENDIX 1 LOW TEMPERATURE (LT) STEELS FOR USE WITH DEP 30.10.02.31-Gen.

The requirements in this appendix relate to the results of Charpy impact tests on full-size
V-notched test pieces (10 mm x 10 mm) tested in accordance with the relevant material
specification. The orientation of the Charpy impact specimens (transverse or longitudinal)
is optional, unless indicated otherwise in the tables. The minimum specified impact
energy is the average of the results of tests made on three test pieces. At most one result
may be lower, with a minimum value at least 70% of the specified minimum average
value. If sub-size specimens have to be used, the required impact value shall be obtained
by multiplying the value specified for full-size specimens by the relevant factor below:
Specimen Size (mm) Factor
10 x 7.5 0.80
10 x 5.0 0.70

For carbon and carbon-manganese steels, the impact requirements are related to
specified minimum tensile strength, as indicated below:
Specified Minimum Required Impact Energy
UTS Value at the Material
(N/mm2) Specification Impact Test
Temperature
(10 x 10 mm specimen)
(Joules)

< 450  27
 450  40

Where the material specification specifies a testing temperature different from the
standard testing temperatures (0, -20, -30, -40, -50, -60, -80, -100, -120, -196 °C), the LT
Number has been obtained by interpolating on the basis of 1.5 Joules per °C. For
example, 18 Joules at -51 °C may be regarded as 27 Joules at -45 °C, i.e. LT 40.
TABLE 1: PLATES, SHEETS AND STRIP - FINE-GRAINED C-Mn STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A516 Grade 55, S5 < 450 18 -51 LT40  25 mm


18 -51 LT40 25-50 mm
18 -46 LT40 50-75 mm
18 -46 LT40 75-125 mm

Grade 60, S5 < 450 18 -51 LT40  25 mm


18 -46 LT40 25-50 mm
18 -46 LT40 50-75 mm
18 -46 LT40 75-125 mm

Grade 65, S5  450 18 -51 LT30  25 mm


18 -46 LT30 25-50 mm
18 -40 LT20 50-75 mm
18 -32 LT0 75-125 mm

A 537 Class 1, S5  450 20 -62 LT30  25 mm


20 -60 LT30 25-50 mm
20 -60 LT30 50-64 mm

Class 2, S5  450 20 -60 LT40 64-75 mm


20 -46 LT30 75-100 mm

A 622 Grade A, S5 < 450 18 -60 LT50  50 mm


Grade B, S5  450 18 -51 LT30  50 mm

BS

1501 164 360 LT20 < 450 27 -20 LT20  63 mm


400 LT20 < 450 27 -20 LT20  63 mm

223 460 LT15  450 41 -15 LT0  63 mm


490 LT15  450 41 -15 LT0  63 mm

224 400 LT50 < 450 27 -50 LT50  63 mm


430 LT50 < 450 27 -50 LT50  63 mm
460 LT30  450 41 -30 LT30  63 mm
490 LT30  450 41 -30 LT30  63 mm

225 490 LT30  450 47 -30 LT30  63 mm


TABLE 1 (CONT'D): PLATES, SHEETS AND STRIP - FINE-GRAINED C-Mn STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
DIN

17102 TSt E 255 < 450 27 -50 LT50  150 mm
ESt E 255 < 450 30 -50 LT50  150 mm
TSt E 285 < 450 27 -50 LT50  150 mm
ESt E 285 < 450 30 -50 LT50  150 mm
TSt E 315 < 450 27 -50 LT50  150 mm
ESt E 315 < 450 30 -50 LT50  150 mm
TSt E 355  450 47 -20 LT20  150 mm
ESt E 355  450 40 -40 LT40  150 mm
TSt E 380  450 47 -20 LT20  150 mm
ESt E 380  450 40 -40 LT40  150 mm
TSt E 420  450 47 -20 LT20  150 mm
ESt E 420  450 40 -40 LT40  150 mm
TSt E 460 450 47 -20 LT20  150 mm
ESt E 460  450 40 -40 LT40  150 mm

17155 HII < 450 31 0 LT0  150 mm


17 Mn 4 < 450 31 0 LT0 100-150 mm
 450 31 0 LT0  100 mm
19 Mn 6  450 31 0 LT0  150 mm

AFNOR

A36-205 A37 FP < 450 27 -40 LT40


A42 FP < 450 27 -40 LT40
A48 FP  450 40 -40 LT40
A52 FP  450 40 -40 LT40

JIS

G3115 SPV 235 < 450 47 0 LT0  200 mm


SPV 315  450 47 0 LT0  100 mm
SPV 355  450 47 0 LT0  75 mm
TABLE 1 (CONT'D): PLATES, SHEETS AND STRIP - FINE-GRAINED C-Mn STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
JIS

G3126 SLA 235A < 450 Note (1) -5 LT0  20 mm


< 450 Note (1) -10 LT0 20-50 mm
SLA 235B < 450 Note (1) -15 LT0  20 mm
< 450 Note (1) -30 LT30 20-50 mm
SLA 325A < 450 Note (1) -25 LT20  20 mm
< 450 Note (1) -35 LT30 20-32 mm
SLA 325B < 450 Note (1) -45 LT40  20 mm
< 450 Note (1) -55 LT50 20-32 mm

Note (1) Shall be not less than half of the maximum absorbed energy value.
The maximum absorbed energy shall be expressed as the average value of absorbed energy
determined at a temperature at which the percentage brittle fracture of three test pieces becomes
zero. This temperature is generally room temperature, but if the percentage brittle fracture of a test
piece does not become zero then the test shall be carried out at a higher temperature.
TABLE 2: PLATES, SHEETS AND STRIP - Ni STEEL
Rm Charpy-V notch LT Remarks
STEEL SPECIFICATION Impact Requirement Number
N/mm2 Joules °C
ASTM

A203 D, S5  450 18 -101 LT80  50 mm


18 -87 LT80 50-75 mm
E, S5  450 20 -101 LT80  50 mm
20 -87 LT80 50-75 mm

A645, S64  450 34 -170 LT120  50 mm

A353, S55 & S56  450 S55,70 (*) -196 LT196  50 mm


S56,40 (*) -196

A553 Type I, S55 & S56  450 S55,80 (*) -196 LT196  50 mm
S56,50 (*) -196

BS

1501 503  450 27 -100 LT100  50 mm


510  450 54 -196 LT196  50 mm
510N  450 54 -196 LT196  50 mm

DIN

17280 11 Mn Ni 5 3 < 450 40 -60 LT60  70 mm


13 Mn Ni 6 3  450 40 -60 LT60  70 mm
14 Ni Mn 6  450 40 -80 LT80  30 mm
40 -70 LT80 30-50 mm
10 Ni 14  450 40 -100 LT100  30 mm
40 -90 LT80 30-50 mm
40 -85 LT80 50-70 mm
12 Ni 19  450 40 -120 LT120  30 mm
40 -110 LT100 30-50 mm
X 8 Ni 9  450 40 -196 LT196  70 mm

AFNOR

A36-208 0.5 Ni 285 < 450 40 -60 LT60  70 mm


355  450 40 -60 LT60  70 mm
1.5 Ni 285  450 40 -80 LT80  70 mm
355  450 40 -80 LT80  70 mm
3.5 Ni 285  450 40 -100 LT100  70 mm
355  450 40 -100 LT100  70 mm
5 Ni 390  450 40 -120 LT120  70 mm
9 Ni 490  450 40 -196 LT196  50 mm
585  450 40 -196 LT196  50 mm

NOTE: (*) 0.50 mm lateral expansion minimum.


TABLE 2 (CONT'D): PLATES, SHEETS AND STRIP - Ni STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
JIS

G3127 SL3N255  450 21 -101 LT80  50 mm


SL3N275  450 21 -101 LT80  50 mm
SL3N440  450 27 -110 LT100  50 mm
SL5N590  450 41 -130 LT120  50 mm
SL9N520  450 34 -196 LT196  50 mm
SL9N590  450 41 -196 LT196  50 mm
TABLE 3: PLATES, SHEETS AND STRIP - AUSTENITIC STAINLESS STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A240 Type 304 - - LT196


304N - - LT196
304L - - LT196
316 - - LT196
316L - - LT196
S31803 (Note 1) 40 -30 LT30
S32750 (Note 1) 40 -30 LT30
S31254 - - LT196
BS

1501 304 S31 - - LT196


304 S11 - - LT196
316 S31 - - LT196
316 S11 - - LT196
318 S13 (Note 1) 40 -30 LT30
SEW

400 X2CrNiMoN 22 5 3 40 -30 LT30


(Note 1)
DIN

17440 X 5 Cr Ni 18 10 - - LT196
X 2 Cr Ni 19 11 - - LT196
X 5 Cr Ni Mo 17 12 2 - - LT196
X 2 Cr Ni Mo 17 13 2 - - LT196
AFNOR

A36-209 Z7 CN 18-09 - - LT196


Z6 CN 18-09 Az - - LT196
Z3 CN 18-10 - - LT196
Z7 CND 17-11-02 - - LT196
Z3 CND 17-11-02 - - LT196
Z3 CND 22-05 Az 40 -30 LT30
(Note 1)
Z3 CND 25-07 Az 40 -30 LT30
(Note 1)
JIS

G4304 SUS 304 - - LT196


SUS 304N1 - - LT196
SUS 304L - - LT196
SUS 316 - - LT196
SUS 316L - - LT196
SUS 329J2L (Note 1) 40 -30 LT30

Note (1) Duplex Stainless Steel (Note that the Charpy V-notch requirement is supplementary to standard
material specification).
TABLE 4: TUBES AND TUBING - FINE-GRAINED C-Mn STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A179 < 450 - - - Note (1)

A334 Grade 6 < 450 18 -45 LT30

BS

3606 CFS 320 < 450 - - - Note (1)

3603 CFS 430 LT Cat. 2 < 450 27 -50 LT50  25 mm

DIN

17175 St 35.8 < 450 - - - Note (1)


St 45.8 < 450 - - - Note (1)

17173 TT St 35 N < 450 40 -40 LT40  10 mm


TT St 35 V < 450 40 -50 LT50  25 mm
40 -40 LT40 25-40 mm

AFNOR

A49-210 TU 37-B < 450 - - - Note (1)


A49-213 TU 37-C < 450 - - - Note (1)
A49-215 TU 37-C < 450 - - - Note (1)
A49-215 TU 42 BT < 450 28 -45 LT40
A49-230 TU 42 BT < 450 28 -45 LT40

JIS

G3461 STB 340 < 450 - - - Note (1)


G3464 STBL 380 < 450 21 -45 LT40

Note (1) Refer to DEP 30.10.02.31-Gen.


TABLE 5: TUBES AND TUBING - Ni STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
BS

3603 CFS 503 LT Cat. 2 < 450 27 -100 LT100


CFS 509 LT Cat. 2  450 40 -196 LT196

DIN

17173 11 Mn Ni 5 3 < 450 40 -60 LT60


13 Mn Ni 6 3  450 40 -60 LT60
10 Ni 14  450 40 -100 LT100  25 mm
40 -90 LT80 25-40 mm
12 Ni 19  450 40 -120 LT120  25 mm
40 -110 LT100 25-40 mm
X 8 Ni 9  450 40 -196 LT196

AFNOR

A49-230 TU 17 N2 > 450 40 -60 LT60


TU 10 N9  450 40 -90 LT80
TU 10 N14  450 40 -100 LT100
TU Z6 N9 > 450 50 -196 LT196

JIS

G3464 STBL 450  450 21 -100 LT80


STBL 690  450 21 -196 LT120
TABLE 6: TUBES AND TUBING - AUSTENITIC STAINLESS STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A249 Type 304 - - LT196


304L - - LT196
316 - - LT196
316L - - LT196

A213 Type 304 - - LT196


304L - - LT196
316 - - LT196
316L - - LT196

BS

3605 LWHT 304 S31 - - LT196


LWHT 304 S11 - - LT196
LWHT 316 S31 - - LT196
LWHT 316 S11 - - LT196

3606 LWHT 304 S31 - - LT196


LWHT 304 S11 - - LT196
LWHT 316 S31 - - LT196
LWHT 316 S11 - - LT196

CFS 304 S31 - - LT196


CFS 304 S11 - - LT196
CFS 316 S31 - - LT196
CFS 316 S11 - - LT196

DIN

17457 X5 Cr Ni 18 10 - - LT196
X2 Cr Ni 19 11 - - LT196
X5 Cr Ni Mo 17 12 2 - - LT196
X2 Cr Ni Mo 17 13 2 - - LT196

17458 X5 Cr Ni 18 10 - - LT196
X2 Cr Ni 19 11 - - LT196
X5 Cr Ni Mo 17 12 2 - - LT196
X2 Cr Ni Mo 17 13 2 - - LT196

AFNOR

A49-217 TUZ6 CN 18-09 - - LT196


TUZ2 CN 18-10 - - LT196
TUZ6 CND 17-11 - - LT196
TUZ2 CND 17-12 - - LT196
TABLE 6 (CONT'D): TUBES AND TUBING - AUSTENITIC STAINLESS STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
AFNOR

A49-214 GRADE DESIGNATION - - LT196


EQUIVALENT TO 304
GRADE DESIGNATION - - LT196
EQUIVALENT TO 304L
GRADE DESIGNATION - - LT196
EQUIVALENT TO 316
GRADE DESIGNATION - - LT196
EQUIVALENT TO 316L

A49-230 TUZ6 CN 19-10 - - LT196


TUZ2 CN 19-11 - - LT196
TUZ6 CND 17-12 - - LT196
TUZ2 CND 17-12 - - LT196

JIS

G3463 SUS 304TB - - LT196 Note (1)


SUS 304LTB - - LT196 Note (1)
SUS 316TB - - LT196 Note (1)
SUS 316LTB - - LT196 Note (1)

Note (1) Seamless and welded.


TABLE 7: PIPE - FINE-GRAINED C-Mn STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A333 Grade 6 < 450 18 -45 LT30

A671 Grade CC65  450 18 -51 LT30  25 mm


Class 32, S2 18 -46 LT30 25-50 mm
18 -40 LT20 50-75 mm
18 -32 LT0 75-125 mm

BS

3603 HFS 430 LT Cat. 2 < 450 27 -50 LT50  25 mm

DIN

17173 TT St 35 N < 450 40 -40 LT40  10 mm


TT St 35 V < 450 40 -50 LT50  25 mm
40 -40 LT40 25-40 mm

AFNOR

A49-230 TU 42 BT < 450 28 -45 LT40

JIS

G3460 STPL 380 < 450 21 -45 LT40


TABLE 8: PIPE - Ni STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A333 Grade 3  450 18 -100 LT80


Grade 8  450 Note (1) -196 LT196

BS

3603 HFS 503 LT Cat. 2 < 450 27 -100 LT100


HFS 509 LT Cat. 2  450 40 -196 LT196

DIN

17173 11 Mn Ni 5 3 < 450 40 -60 LT60


13 Mn Ni 6 3  450 40 -60 LT60
10 Ni 14  450 40 -100 LT100  25 mm
40 -90 LT80 25-40 mm
12 Ni 19  450 40 -120 LT120  25 mm
40 -110 LT100 25-40 mm
X 8 Ni 9  450 40 -196 LT196

AFNOR

A49-230 TU 27 N2 > 450 40 -60 LT60


TU 10 N9  450 40 -80 LT80
TU 10 N14  450 40 -100 LT100
TU Z6 N9 > 450 50 -196 LT196

JIS

G3460 STPL 450  450 21 -100 LT80


STPL 690  450 21 -196 LT120

Note (1) 0.38 mm lateral expansion minimum.


TABLE 9: PIPE - AUSTENITIC STAINLESS STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A312 Type 304 - - LT196


304L - - LT196
316 - - LT196
316L - - LT196
S31254 - - LT196

A358 Type 304 Class 1 - - LT196


316 Class 1 - - LT196

A790 S31803 (Note 1) 40 -30 LT30


S32750 (Note 1) 40 -30 LT30

BS

3605 CFS 304 S31 - - LT196


CFS 304 S11 - - LT196
CFS 316 S31 - - LT196
CFS 316 S11 - - LT196

LWHT 304 S31 - - LT196


LWHT 304 S11 - - LT196
LWHT 316 S31 - - LT196
LWHT 316 S11 - - LT196

DIN

17457 X5 Cr Ni 18 10 - - LT196
X2 Cr Ni 19 11 - - LT196
X5 Cr Ni Mo 17 12 2 - - LT196
X2 Cr Ni Mo 17 13 2 - - LT196

17458 X5 Cr Ni 18 10 - - LT196
X2 Cr Ni 19 11 - - LT196
X5 Cr Ni Mo 17 12 2 - - LT196
X2 Cr Ni Mo 17 13 2 - - LT196

AFNOR

A49-230 TUZ6 CN 19-10 - - LT196


TUZ2 CN 19-11 - - LT196
TUZ6 CND 17-12 - - LT196
TUZ2 CND 17-12 - - LT196

JIS

G3459 SUS 304TP - - LT196


SUS 304LTP - - LT196
SUS 316TP - - LT196
SUS 316LTP - - LT196
SUS 329J2LTP (Note 40 -30 LT30
1)
Note (1) Duplex stainless steel (Note that the Charpy V-notch requirement is supplementary to the
standard material specification).
TABLE 10: FORGINGS, FLANGES AND FITTINGS - FINE-GRAINED C-Mn STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A350 LF2  450 20 -45.6 LT30


A420 WPL6 + WPL6W < 450 17.6 -45 LT30
A765 Grade II  450 20 -45 LT30

BS

1503 223-410 LT10 < 450 27 -10 LT0 No limit


LT20 27 -20 LT20  150 mm
LT50 27 -50 LT50  100 mm

223-430 LT10 < 450 27 -10 LT0 No limit


LT15 27 -15 LT0  150 mm
LT40 27 -40 LT40  100 mm

223-460 LT0  450 41 0 LT0 No limit


LT10 41 -10 LT0  150 mm
LT20 41 -20 LT20  100 mm

223-490 LT0  450 41 0 LT0  150 mm


LT10 41 -10 LT0  100 mm

223-510 LT0  450 41 0 LT0  150 mm

224-410 LT10 < 450 27 -10 LT0 No limit


LT20 27 -20 LT20  150 mm
LT50 27 -50 LT50  100 mm

224-430 LT10 < 450 27 -10 LT0 No limit


LT15 27 -15 LT0  150 mm
LT40 27 -40 LT40  100 mm

224-460 LT0  450 41 0 LT0 No limit


LT10 41 -10 LT0  150 mm
LT20 41 -20 LT20  100 mm

224-490 LT0  450 41 0 LT0  150 mm


LT10 41 -10 LT0  100 mm

224-510 LT0  450 41 0 LT0  150 mm

1640 WPL 0 < 450 21 -50 LT40

JIS

G3205 SFL 2  450 27 -45 LT30


TABLE 11: FORGINGS, FLANGES AND FITTINGS - Ni STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A420 WPL 3 + WPL3W  450 17.6 -100 LT80


WPL 8 + WPL8W  450 33.9 -196 LT196

A350 LF 3  450 20 -101 LT80

A522 Type I (NNT)  450 L 70 (*) -196 LT196  75 mm


T 40 (*) -196

Type I (QT)  450 L 80 (*) -196 LT196  125 mm


T 50 (*) -196

BS

1640 WPL 3  450 21 -100 LT80

1503 503-490  450 27 -80 LT80  150 mm


509-690  450 34 -196 LT196  150 mm

DIN

17280 11 Mn Ni 5 3 < 450 40 -60 LT60  70 mm


13 Mn Ni 6.3  450 40 -60 LT60  70 mm
14 Ni Mn 6  450 40 -80 LT80  30 mm
40 -70 LT60 30-50 mm
10 Ni 14  450 40 -100 LT100  30 mm
40 -90 LT80 30-50 mm
40 -85 LT80 50-70 mm
12 Ni 19  450 40 -120 LT120  30 mm
40 -110 LT100 30-50 mm
X 8 Ni 9  450 40 -196 LT196  70 mm

JIS

G3205 SFL 3  450 27 -101 LT100

NOTE (*) 0.50 mm lateral expansion minimum


where L = Longitudinal axis of specim en oriented parallel to major direction of grain flow.
and T = Longitudinal axis of specim en oriented transverse to major direction of grain flow.
(Testing to be carried out in both directions)
TABLE 12: FORGINGS, FLANGES AND FITTINGS - AUSTENITIC STAINLESS
STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A403 WP 304 - - LT196


WP 304L - - LT196
WP 316 - - LT196
WP 316L - - LT196
WP S31254 - - LT 196

A815 S31803 (Note 1) 40 -30 LT30


Class WP-S or
WP-WK

A182 F 304 - - LT196


F 304L - - LT196
F 316 - - LT196
F 316L - - LT196
F 44 - - LT196
F 51 (Note 1) 40 -30 LT30
F 53 (Note 1) 40 -30 LT30
BS

1640 WP 304 - - LT196


WP 304L - - LT196
WP 316 - - LT196
WP 316L - - LT196

1503 304 S31 - - LT196


304 S11 - - LT196
316 S31 - - LT196
316 S11 - - LT196
318 S13 (Note 1) 40 -30 LT30

970 304 S31 - - LT196


304 S11 - - LT196
316 S31 - - LT196
316 S11 - - LT196
SEW

400 X2CrNiMoN 225 3 40 -30 LT30


(Note 1)
DIN

17440 X5 Cr Ni 18 10 - - LT196
X2 Cr Ni 19 11 - - LT196
X5 Cr Ni Mo 17 12 2 - - LT196
X2 Cr Ni Mo 17 13 2 - - LT196

Note (1) Duplex stainless steel (Note that the Charpy V-notch requirement is supplementary to standard
material specification).
TABLE 12 (CONT'd): FORGINGS, FLANGES AND FITTINGS - AUSTENITIC
STAINLESS STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
AFNOR

A36-607 Z6 CN 18-09 - - LT196


Z2 CN 18-10 - - LT196
Z6 CND 17-11 - - LT196
Z2 CND 17-12 - - LT196

JIS

G3214 SUS F304 - - LT196


SUS F304L - - LT196
SUS F316 - - LT196
SUS F316L - - LT196
TABLE 13: CASTINGS - FINE-GRAINED C-Mn STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A352 LCA < 450 18 -32 LT20


LCB  450 18 -46 LT30
LCC  450 20 -46 LT30

BS

1504 161-430A LT40 < 450 20 -40 LT30

SEW

685 GS-21 Mn 5 N  450 27 -30 LT20  30 mm


GS-21 Mn 5  450 35 -50 LT40  100 mm

AFNOR

A32-055 A420 FP-M  450 22 -40 LT30


A480 FP-M > 450 24 -40 LT30

JIS

G5152 SCPL 1  450 18 -45 LT30


TABLE 14: CASTINGS - Ni STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A352 LC 3  450 20 -101 LT80


LC 9  450 27 -196 LT196

A571 D-2M Class 1 (Note 1) - 21 -196 LT100


Class 2 (Note 1) - 27 -196 LT100

BS

1504 503 LT60  450 20 -60 LT40

3468 S2M (Note 1) - 15 -150 LT100

SEW

685 GS-10 Ni 6 < 450 27 -50 LT50


GS-10 Ni 14  450 27 -90 LT80

DIN

1694 GGG-Ni Mn 23 4 < 450 24 -196 LT100


(Note 1)

AFNOR

A32-053 FC3-M  450 22 -40 LT30


A32-055 20N12-M > 450 24 -40 LT30
A32-301 S-NM 23 4 (Note 1) < 450 27 -100 LT100

JIS

G3152 SCPL 31  450 21 -100 LT80

Note (1) Austenitic ductile Iron


TABLE 15: CASTINGS - AUSTENITIC STAINLESS STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A351 CF8 - - LT196


CF8M - - LT196

A744 CF8 - - LT196


CF8M - - LT196

BS

1504 304 C15 LT196 41 -196 LT196


316 C16 LT196 41 -196 LT196

3100 304 C15 41 -196 LT196


316 C16 41 -196 LT196

DIN

17445 G-X 6 Cr Ni 18 9 - - LT196


G-X 6 Cr Ni Mo 18 10 - - LT196

AFNOR

A32-056 Z6 CN 18-10-M - - LT196


Z6 CND 18-12-M - - LT196

JIS

G5121 SCS 13A - - LT196


SCS 14A - - LT196
TABLE 16: BARS, SECTIONS AND WIRE - FINE-GRAINED C-Mn STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
BS

1502 211 LT0 < 450 27 0 LT0


221 LT0 < 450 27 0 LT0
224 430 LT50 < 450 27 -50 LT50
224 490 LT30  450 41 -30 LT30

DIN

17102 TSt E 255 < 450 27 -50 LT50  150 mm


ESt E 255 < 450 30 -50 LT50  150 mm
TSt E 285 < 450 27 -50 LT50  150 mm
ESt E 285 < 450 30 -50 LT50  150 mm
TSt E 315 < 450 27 -50 LT50  150 mm
ESt E 315 < 450 30 -50 LT50  150 mm
TSt E 355  450 47 -20 LT20  150 mm
ESt E 355  450 40 -40 LT40  150 mm
TSt E 380  450 47 -20 LT20  150 mm
ESt E 380  450 40 -40 LT40  150 mm
TSt E 420  450 47 -20 LT20  150 mm
ESt E 420  450 40 -40 LT40  150 mm
TSt E 460  450 47 -20 LT20  150 mm
ESt E 460  450 40 -40 LT40  150 mm
TSt E 500  450 47 -20 LT20  150 mm
ESt E 500  450 40 -40 LT40  150 mm
TABLE 17: BARS, SECTIONS AND WIRE - Ni STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
BS

1502 509-650  450 42 -196 LT196


509-690  450 27 -196 LT196

DIN

17280 11 Mn Ni 5 3 < 450 40 -60 LT60


13 Mn Ni 6 3  450 40 -60 LT60
14 Ni Mn 6  450 40 -80 LT80  30 mm
40 -70 LT60 30-50 mm
10 Ni 14 450 40 -100 LT100  30 mm
40 -90 LT80 30-50 mm
40 -80 LT80 50-70 mm
12 Ni 19 450 40 -120 LT120  30 mm
40 -110 LT100 30-50 mm
X 8 Ni 9 450 40 -196 LT196
TABLE 18: BARS, SECTIONS AND WIRE - AUSTENITIC STAINLESS STEEL
Rm Charpy V-notch LT Remarks
STEEL SPECIFICATION Impact Number
Requirement
N/mm2 Joules °C
ASTM

A276 S 31254 - - LT196

A479 Type 304 - - LT196


Type 304L - - LT196
Type 316 - - LT196
Type 316L - - LT196
S 31803 (Note 1) 40 -30 LT30
S 32750 (Note 1) 40 -30 LT30

A313 Type 302 - - LT196

BS

970 304 S15 - - LT196


316 S31 - - LT196

1502 304 S11 - - LT196


304 S31 - - LT196
316 S11 - - LT196
316 S31 - - LT196

2056 302 S26 - - LT196

DIN

17440 X 5 Cr Ni 18 10 - - LT196
X 2 Cr Ni 19 11 - - LT196
X 5 Cr Ni Mo 17 12 2 - - LT196
X 2 Cr Ni Mo 17 13 2 - - LT196

17224 X 12 Cr Ni 17 7 - - LT196

AFNOR

A35-574 Z6 CN 18-09 - - LT196


Z7 CND 17-11-02 - - LT196
Z12 CN 18-09 - - LT196

JIS

G4303 SUS 304 - - LT196


SUS 316 - - LT196

G4314 SUS 302 - - LT196

Note (1) Duplex stainless steel (Note that the Charpy V-notch requirem ent is supplementary to standard
material specification).
TABLE 19: BOLTING
Charpy-V notch Minimum Remarks
STEEL SPECIFICATON Impact Allowable
Requirement Lower Design
Temperature
BOLTS NUTS Joules °C °C
ASTM

A193 B7 A194 2H - - -30  40 mm dia.


B7M 2HM - - -30  40 mm dia.
B8 Class 1 8 - - -200
B8 Class 2 8,S1 - - -200
B8T Class 1 8T - - -200
B8T Class 2 8T,S1 - - -200
B8C Class 1 8C - - -200
B8C Class 2 8C,S1 - - -200
B8M Class 1 8M - - -200
B8M Class 2 8M,S1 - - -200
B8N Class 1 8N - - -200
B8N Class 2 8N,S1 - - -200

A320 L7 A194 4,S4 27 -101 -105


L7M 7M,S4 27 -73 -80
B8 Class 1 8 - - -200
B8 Class 2 8,S1 - - -200
B8T Class 1 8T - - -200
B8T Class 2 8T,S1 - - -200
B8C Class 1 8C - - -200
B8C Class 2 8C,S1 - - -200
B8M Class 1 8M - - -200
B8M Class 2 8M,S1 - - -200
B8N Class 1 8N - - -200
B8N Class 2 8N,S1 - - -200

BS

4882 B7 4882 2H - - -30  40 mm dia.


B7M 2HM - - -30  40 mm dia.
L7 L4 27 -100 -105
L7M L7M 27 -100 -105
L9 L9 40 -196 -200
L9A L9A 40 -196 -200
B8 8 - - -200
B8X 8X - - -200
B8T 8T - - -200
B8C 8C - - -200
B8M 8M - - -200
B8MX 8MX - - -200
B8N 8N - - -200
TABLE 19: BOLTING (CONT'D)
Charpy V-notch Minimum Remarks
STEEL SPECIFICATION Impact Allowable
Requirement Lower Design
Temperature
BOLTS NUTS Joules °C °C
DIN

17200: 17200:
42 Cr Mo 4 C45 - - -30  40 mm dia.

17440: 17440:
X 5 CrNi 18 10 X 5 CrNi18 10 - - -200
X 6 CrNiTi 18 10 X 6 CrNiTi 18 10 - - -200
X 6 CrNiNb 18 10 X 6 CrNiNb 18 10 - - -200
X 5 CrNiMo 17 12 2 X 5 CrNiMo 17 12 2 - - -200

AFNOR

A35-557 42 CD 4 A35-557 XC 38 - - -30  40 mm dia.

A35-559 42 CD 4 A35-559 42 CD 4 28 -50 -50

A35-574 A35-574
Z6 CN 18-09 Z6 CN 18-09 - - -200
Z6 CNT 18-10 Z6 CNT 18-10 - - -200
Z7 CND 17-11-02 Z7 CND 17-11-02 - - -200

JIS

G4107 SNB7 G4051 S43C - - -30  40 mm dia.

G4303 SUS 304 G4303 SUS 304 - - -200


SUS 321 SUS 321 - - -200
SUS 347 SUS 347 - - -200
SUS 316 SUS 316 - - -200
SUS 304N1 SUS 304N1 - - -200

You might also like